WO2009116302A1 - Flame-retardant polyester resin composition and flame-retardant laminate - Google Patents
Flame-retardant polyester resin composition and flame-retardant laminate Download PDFInfo
- Publication number
- WO2009116302A1 WO2009116302A1 PCT/JP2009/001253 JP2009001253W WO2009116302A1 WO 2009116302 A1 WO2009116302 A1 WO 2009116302A1 JP 2009001253 W JP2009001253 W JP 2009001253W WO 2009116302 A1 WO2009116302 A1 WO 2009116302A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- layer
- polyester resin
- melamine
- laminate
- flame retardant
- Prior art date
Abstract
Description
リン系化合物も考えられるが、安全性や環境調和性の点で課題があるばかりか、特にポリエステル系樹脂にリン系化合物を配合すると、可塑化による耐熱性の低下や、リン系化合物の成形品表面へのブリードが生じるため、実用上好ましい技術と言うことはできない。 As flame retardants for polyester resins, halogen flame retardants such as decabromodiphenyl ether and hexabromodiphenyl have been used. Halogen flame retardants generate harmful gases such as dioxins during combustion. In some cases, it is also a problem in terms of safety during waste incineration and thermal recycling.
Phosphorus compounds are also conceivable, but not only are there problems in terms of safety and environmental harmony, but especially when a phosphorus compound is added to a polyester resin, the heat resistance decreases due to plasticization, and the molded product of the phosphorus compound. Since bleeding to the surface occurs, it cannot be said to be a practically preferable technique.
窒素系化合物、特にメラミンを難燃化剤として用いる点については、例えば特開昭54-112958号公報、特公昭60-33850号公報、特公昭59-50184号公報、特公昭62-39174号公報などに記載されている。 Therefore, the present inventor has focused on nitrogen compounds, particularly melamine, as non-halogen / non-phosphorus flame retardants used in polyester resins.
Regarding the use of nitrogen-based compounds, particularly melamine, as a flame retardant, for example, JP-A-54-12958, JP-B-60-33850, JP-B-59-50184, JP-B-62-39174 It is described in.
このような特定のポリエステル系樹脂に対してメラミンを配合することで、ポリエステル系樹脂が本来有する特性を損なうことなく、従来検討されてきた無機系難燃剤よりも低添加量で、かつ、優れた難燃性、機械特性、耐熱性を得ることができる。 Polyester resins having a glass transition temperature Tg of 40 ° C. or lower and a crystal melting temperature Tm of 140 ° C. to 190 ° C. have a lower melting point than ordinary polyester resins such as PET and PBT, and melamine decomposes. Since molding is possible at a temperature lower than the temperature, it is possible to eliminate the occurrence of molding defects due to decomposition of melamine during molding. In addition, excellent flexibility and mechanical properties can be obtained.
By adding melamine to such a specific polyester-based resin, the added amount is lower than that of the inorganic flame retardants that have been studied so far, without impairing the inherent properties of the polyester-based resin. Flame retardancy, mechanical properties, and heat resistance can be obtained.
第1の実施形態に係る難燃性ポリエステル系樹脂組成物(以下「第1の難燃性樹脂組成物」という)について説明する。 [First Embodiment]
The flame-retardant polyester resin composition according to the first embodiment (hereinafter referred to as “first flame-retardant resin composition”) will be described.
第1の難燃性樹脂組成物は、ポリエステル系樹脂(1-A)及びメラミンの混合物を含有する難燃性ポリエステル系樹脂組成物であり、好ましくはさらにポリエステル系樹脂(1-B)を含有する難燃性ポリエステル系樹脂組成物である。 <Composition of the first flame retardant resin composition>
The first flame retardant resin composition is a flame retardant polyester resin composition containing a mixture of a polyester resin (1-A) and melamine, and preferably further contains a polyester resin (1-B). It is a flame retardant polyester resin composition.
ポリエステル系樹脂(1-A)は、多価カルボン酸と多価アルコールとの重縮合ポリマーであるポリエステル系樹脂である。
多価カルボン酸の具体例としては、例えばテレフタル酸、イソフタル酸、コハク酸、アジピン酸、セバシン酸、ドデカン二酸等を挙げることができる。
多価アルコールの具体例としては、例えばエチレングリコール、プロピレングリコール、1,4-ブタンジオール、1,6-ヘキサンジオール、シクロヘキサンジオール、ポリオキシレングリコール、ポリテトラメチレンエーテルグリコール等を挙げることができる。
中でも、テレフタル酸、イソフタル酸、及びアジピン酸から選ばれる少なくとも1種類の多価カルボン酸成分と、1,4-ブタンジオール及びエチレングリコールから選ばれる少なくとも1種類の多価アルコール成分とからなる共重合体であるのが好ましい。 (Polyester resin (1-A))
The polyester resin (1-A) is a polyester resin that is a polycondensation polymer of a polyvalent carboxylic acid and a polyhydric alcohol.
Specific examples of the polyvalent carboxylic acid include terephthalic acid, isophthalic acid, succinic acid, adipic acid, sebacic acid, dodecanedioic acid and the like.
Specific examples of the polyhydric alcohol include ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, cyclohexanediol, polyoxylene glycol, polytetramethylene ether glycol and the like.
Among these, a co-polymer comprising at least one polycarboxylic acid component selected from terephthalic acid, isophthalic acid, and adipic acid and at least one polyhydric alcohol component selected from 1,4-butanediol and ethylene glycol. It is preferably a coalescence.
かかる観点から、ポリエステル系樹脂(1-A)は、多価カルボン酸成分として、テレフタル酸を55mol%以上、特に60mol%以上含有するのがさらに好ましく、又、85mol%以下、特に80mol%以下含有するのがさらに好ましい。
但し、多価カルボン酸成分中に占めるテレフタル酸の割合が50~90mol%であるポリエステル系樹脂に限定する趣旨ではない。 In the polyester resin (1-A), the proportion of terephthalic acid in the polyvalent carboxylic acid component is preferably 50 to 90 mol%. The polyester resin (1-A) having such a composition has a lower melting point than general polyester resins such as PET and PBT, and can be molded at a temperature lower than the temperature at which melamine starts to decompose. Therefore, it is possible to eliminate the occurrence of molding defects due to decomposition of melamine during molding. In addition, excellent flexibility and mechanical properties can be obtained.
From this point of view, the polyester resin (1-A) preferably contains terephthalic acid as a polyvalent carboxylic acid component in an amount of 55 mol% or more, particularly 60 mol% or more, and more preferably 85 mol% or less, particularly 80 mol% or less. More preferably.
However, it is not intended to limit the polyester resin in which the proportion of terephthalic acid in the polyvalent carboxylic acid component is 50 to 90 mol%.
かかる観点から、ポリエステル系樹脂(1-A)は、多価アルコール成分として、1,4-ブタンジオール及びエチレングリコールを合計で75mol%以上、特に80mol%以上含有するのが好ましく、100mol%含有するのがさらに好ましい。
但し、多価アルコール成分としては、1,4-ブタンジオール、エチレングリコール及びジエチレングリコールのうちのいずれか一種を含んでいてもよいし、2種以上を含んでいてもよい。 The polyester resin (1-A) preferably contains 70 to 100 mol% of the total proportion of 1,4-butanediol and ethylene glycol in the polyhydric alcohol component. With the polyester resin (1-A) having such a composition, excellent flexibility, mechanical properties, and heat resistance can be obtained.
From this point of view, the polyester resin (1-A) contains 1,4-butanediol and ethylene glycol as a polyhydric alcohol component in a total amount of 75 mol% or more, particularly preferably 80 mol% or more, and preferably 100 mol%. Is more preferable.
However, the polyhydric alcohol component may include any one of 1,4-butanediol, ethylene glycol, and diethylene glycol, or may include two or more.
かかる観点から、ポリエステル系樹脂(1-A)の質量平均分子量は、特に20,000以上、中でも特に30,000以上であるのがさらに好ましく、特に200,000以下、中でも特に150,000以下であるのがさらに好ましい。 The mass average molecular weight of the polyester resin (1-A) is preferably 10,000 to 300,000. If the mass average molecular weight of the polyester-based resin (1-A) is within such a range, flexibility can be obtained, and the melt viscosity is appropriate, so that there is little possibility of problems in molding.
From this point of view, the mass average molecular weight of the polyester-based resin (1-A) is particularly preferably 20,000 or more, more preferably 30,000 or more, particularly 200,000 or less, especially 150,000 or less. More preferably.
ゲルパーミエーションクロマトグラフィーを用いて、溶媒クロロホルム、溶液濃度0.2wt/vol%、溶液注入量200μL、溶媒流速1.0ml/分、溶媒温度40℃で測定を行い、ポリスチレン換算で質量平均分子量を算出することができる。この際に用いる標準ポリスチレンの質量平均分子量は、2,000,000、430,000、110,000、35,000、10,000、40,00、600である。 The mass average molecular weight can be measured by the following method. The same applies to other resins.
Using gel permeation chromatography, measurement is made at a solvent chloroform, a solution concentration of 0.2 wt / vol%, a solution injection amount of 200 μL, a solvent flow rate of 1.0 ml / min, a solvent temperature of 40 ° C., and a mass average molecular weight in terms of polystyrene is obtained. Can be calculated. The mass average molecular weight of the standard polystyrene used in this case is 2,000,000, 430,000, 110,000, 35,000, 10,000, 40,00, 600.
ポリエステル系樹脂(1-B)は、多価カルボン酸と多価アルコールとの重縮合ポリマーであるポリエステル系樹脂である。 (Polyester resin (1-B))
The polyester resin (1-B) is a polyester resin that is a polycondensation polymer of a polyvalent carboxylic acid and a polyhydric alcohol.
多価アルコールの具体例としては、例えばエチレングリコール、プロピレングリコール、1,4-ブタンジオール、1,6-ヘキサンジオール、シクロヘキサンジオール、ポリオキシレングリコール、ポリテトラメチレンエーテルグリコール等を挙げることができる。
中でも、テレフタル酸、イソフタル酸、及びアジピン酸から選ばれる少なくとも1種類の多価カルボン酸成分と、1,4-ブタンジオール及びエチレングリコールから選ばれる少なくとも1種類の多価アルコール成分とからなる共重合体であるのが好ましい。 Specific examples of the polyvalent carboxylic acid include terephthalic acid, isophthalic acid, succinic acid, adipic acid, sebacic acid, dodecanedioic acid and the like.
Specific examples of the polyhydric alcohol include ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, cyclohexanediol, polyoxylene glycol, polytetramethylene ether glycol and the like.
Among these, a co-polymer comprising at least one polycarboxylic acid component selected from terephthalic acid, isophthalic acid, and adipic acid and at least one polyhydric alcohol component selected from 1,4-butanediol and ethylene glycol. It is preferably a coalescence.
このような組成を有するポリエステル系樹脂(1-B)を、前記ポリエステル系樹脂(1-A)と共に配合すれば、柔軟性、特に優れた伸びを得ることができて好ましい。かかる観点から、ポリエステル系樹脂(1-B)は、多価カルボン酸成分として、テレフタル酸を30mol%以上、特に40mol%以上含有するのがさらに好ましく、また、65mol%未満、特に60mol%未満含有するのがさらに好ましい。
但し、多価カルボン酸成分中に占めるテレフタル酸の割合が20mol%以上70mol%未満であるポリエステル系樹脂に限定する趣旨ではない。 In the polyester resin (1-B), the proportion of terephthalic acid in the polyvalent carboxylic acid component is preferably 20 mol% or more and less than 70 mol%.
It is preferable to blend the polyester-based resin (1-B) having such a composition with the polyester-based resin (1-A) because flexibility and particularly excellent elongation can be obtained. From this point of view, the polyester resin (1-B) further preferably contains terephthalic acid as a polyvalent carboxylic acid component in an amount of 30 mol% or more, particularly 40 mol% or more, and less than 65 mol%, particularly less than 60 mol%. More preferably.
However, it is not intended to limit the polyester-based resin in which the proportion of terephthalic acid in the polyvalent carboxylic acid component is 20 mol% or more and less than 70 mol%.
かかる観点から、ポリエステル系樹脂(1-B)は、多価アルコール成分として、1,4-ブタンジオール及びエチレングリコールを合計で70mol%以上、特に75mol%以上含有するのが好ましく、また、特に95mol%以下、中でも90mol%含有するのがさらに好ましい。
但し、多価アルコール成分としては、1,4-ブタンジオール、エチレングリコール及びジエチレングリコールのうちのいずれか一種を含んでいてもよいし、2種以上を含んでいてもよい。 In the polyester resin (1-B), the total proportion of 1,4-butanediol and ethylene glycol in the polyhydric alcohol component is preferably 65 to 100 mol%. When the polyester resin (1-B) having such a composition is blended with the polyester resin (1-A), the mechanical properties are further improved without impairing the heat resistance of the polyester resin (1-A). can do.
From this point of view, the polyester resin (1-B) preferably contains a total of 1,4-butanediol and ethylene glycol as polyhydric alcohol components of 70 mol% or more, particularly 75 mol% or more, and particularly 95 mol%. % Or less, more preferably 90 mol%.
However, the polyhydric alcohol component may include any one of 1,4-butanediol, ethylene glycol, and diethylene glycol, or may include two or more.
かかる観点から、ポリエステル系樹脂(1-B)の質量平均分子量は、特に20,000以上、中でも特に30,000以上であるのがさらに好ましく、特に200,000以下、中でも特に150,000以下であるのがさらに好ましい。 The mass average molecular weight of the polyester resin (1-B) is preferably 10,000 to 300,000. If the mass average molecular weight of the polyester-based resin (1-B) is within such a range, flexibility can be obtained, and the melt viscosity is appropriate, so that there is little possibility of problems in molding.
From this viewpoint, the mass average molecular weight of the polyester-based resin (1-B) is particularly preferably 20,000 or more, more preferably 30,000 or more, particularly 200,000 or less, especially 150,000 or less. More preferably.
ゲルパーミエーションクロマトグラフィーを用いて、溶媒クロロホルム、溶液濃度0.2wt/vol%、溶液注入量200μL、溶媒流速1.0ml/分、溶媒温度40℃で測定を行い、ポリスチレン換算で質量平均分子量を算出することができる。この際に用いる標準ポリスチレンの質量平均分子量は、2000000、430000、110000、35000、10000、4000、600である。 The mass average molecular weight can be measured by the following method. The same applies to other resins.
Using gel permeation chromatography, measurement is made at a solvent chloroform, a solution concentration of 0.2 wt / vol%, a solution injection amount of 200 μL, a solvent flow rate of 1.0 ml / min, a solvent temperature of 40 ° C., and a mass average molecular weight in terms of polystyrene is obtained. Can be calculated. The mass average molecular weight of the standard polystyrene used in this case is 20000, 430000, 110000, 35000, 10000, 4000, 600.
メラミンとは、構造の中心にトリアジン環を持つ有機窒素化合物の一種であり、例えば2,4,6-トリアミノ-1,3,5-トリアジンを挙げることができる。メラミンは、燃焼時に不燃性のガスを発生するため、第1の難燃性樹脂組成物を難燃化することができる。
メラミンは、分解開始温度がメラミンの誘導体(例えば、メラミンシアヌレート、リン酸メラミン等)と比較して低く、また、炭化促進作用もないため、一般的には難燃剤として用いることは困難であるが、本発明のポリエステル系樹脂(1-A)、或いはポリエステル系樹脂(1-A)及び(1-B)に配合することで、メラミンの分解開始温度以下で溶融混練可能であり、かつ、燃焼時においては、樹脂の分解よりも先にメラミンが分解することで、昇華時の吸熱作用、及び、不活性ガスの発生により、優れた難燃性を付与することが可能である。 (melamine)
Melamine is a kind of organic nitrogen compound having a triazine ring at the center of the structure, and examples thereof include 2,4,6-triamino-1,3,5-triazine. Since melamine generates nonflammable gas at the time of combustion, the first flame retardant resin composition can be made flame retardant.
Melamine has a lower decomposition initiation temperature than melamine derivatives (for example, melamine cyanurate, melamine phosphate, etc.) and has no carbonization promoting action, so it is generally difficult to use as a flame retardant. However, by blending with the polyester resin (1-A) or the polyester resins (1-A) and (1-B) of the present invention, it can be melt-kneaded at a temperature lower than the decomposition start temperature of melamine, and At the time of combustion, melamine is decomposed prior to the decomposition of the resin, so that excellent flame retardancy can be imparted by the endothermic action during sublimation and generation of inert gas.
なお、前記平均粒径は、メラミンを円相当径として計算した値である。 The average particle size of melamine is preferably 10 μm or less, particularly 0.5 μm to 10 μm. If the average particle size of the melamine is within this range, the melamine does not agglomerate and is uniformly dispersed in the resin composition. Therefore, the flame retardancy is not impaired without impairing the mechanical strength of the first flame retardant resin composition. Can be improved. From this point of view, the average particle size of melamine is particularly preferably 1.0 μm or more, particularly preferably 1.5 μm or more, particularly preferably 8.0 μm or less, and particularly preferably 6.0 μm or less.
The average particle diameter is a value calculated by using melamine as the equivalent circle diameter.
表面処理の具体例としては、エポキシシラン、ビニルシラン、メタクリルシラン、アミノシラン、イソシアネートシラン等のシランカップリング剤、チタネートカップリング剤、高級脂肪酸等を用いた表面処理を挙げることができる。
これらの表面処理剤でメラミンを処理することによって、メラミンの分散性を向上し、第1の難燃性樹脂組成物の難燃性をさらに向上させることができる。 A surface treatment can be applied to melamine as long as the effects of the present invention are not impaired.
Specific examples of the surface treatment include surface treatment using a silane coupling agent such as epoxy silane, vinyl silane, methacryl silane, amino silane, isocyanate silane, titanate coupling agent, higher fatty acid and the like.
By treating melamine with these surface treatment agents, the dispersibility of melamine can be improved and the flame retardancy of the first flame retardant resin composition can be further improved.
他の難燃剤の具体例としては、例えばリン酸エステル、リン酸エステルアミド、縮合リン酸エステル、ホスファゼン化合物、ポリリン酸塩等のリン系化合物、水酸化アルミニウム、水酸化マグネシウム、カルシウム・アルミネート水和物、酸化スズ水和物等の金属水酸化物を挙げることができる。
難燃助剤の具体例としては、例えばスズ酸亜鉛、ホウ酸亜鉛、硝酸鉄、硝酸銅、スルホン酸金属塩等の金属化合物、ジメチルシリコーン、フェニルシリコーン、フッ素シリコーン等のシリコーン化合物、ポリテトラフルオロエチレン等のフッ素化合物を挙げることができる。
これらの難燃剤、難燃助剤を併用することで、第1の難燃性樹脂組成物の難燃性をさらに向上することができる。 In addition, melamine and other flame retardants or flame retardant aids may be used in combination as long as the effects of the present invention are not impaired.
Specific examples of other flame retardants include, for example, phosphoric acid esters, phosphoric acid ester amides, condensed phosphoric acid esters, phosphazene compounds, phosphorus compounds such as polyphosphates, aluminum hydroxide, magnesium hydroxide, calcium aluminate water Examples thereof include metal hydroxides such as hydrates and tin oxide hydrates.
Specific examples of flame retardant aids include, for example, metal compounds such as zinc stannate, zinc borate, iron nitrate, copper nitrate, and sulfonic acid metal salts, silicone compounds such as dimethyl silicone, phenyl silicone, and fluorine silicone, polytetrafluoro Fluorine compounds such as ethylene can be mentioned.
By using these flame retardants and flame retardant aids in combination, the flame retardancy of the first flame retardant resin composition can be further improved.
第1の難燃性樹脂組成物中に占めるメラミンの配合割合は、20~60質量%であるのが好ましい。第1の難燃性樹脂組成物中に占めるメラミンの配合割合が20質量%以上であれば、十分な難燃性を得ることができる一方、メラミンの配合割合が60質量%以下であれば機械物性を損なうことがない。かかる観点から、第1の難燃性樹脂組成物中に占めるメラミンの配合割合は、20質量%以上であるのが特に好ましく、中でも30質量%以上であるのがさらに好ましい。また、50質量%以下であるのが特に好ましく、中でも40質量%以下であるのがさらに好ましい。 (Mixing ratio)
The blending ratio of melamine in the first flame retardant resin composition is preferably 20 to 60% by mass. If the blending ratio of melamine in the first flame-retardant resin composition is 20% by mass or more, sufficient flame retardancy can be obtained, while if the blending ratio of melamine is 60% by mass or less, the machine There is no loss of physical properties. From such a viewpoint, the blending ratio of melamine in the first flame retardant resin composition is particularly preferably 20% by mass or more, and more preferably 30% by mass or more. Moreover, it is especially preferable that it is 50 mass% or less, and it is still more preferable that it is 40 mass% or less especially.
かかる観点から、ポリエステル系樹脂(1-A)とポリエステル系樹脂(1-B)の混合割合は、特にポリエステル系樹脂(1-B)が80:20以上、中でも70:30以上の割合で含まれるようにポリエステル系樹脂(1-B)を混合するのが好ましい一方、ポリエステル系樹脂(1-B)が40:60以下、中でも50:50以下の割合で含まれるようにポリエステル系樹脂(1-B)を混合するのが好ましい。 When the polyester resin (1-B) is blended, the mixing ratio of the polyester resin (1-A) and the polyester resin (1-B) is 90:10 to 30:70 by mass ratio. Is preferred. With such a ratio, the mechanical properties can be further improved without impairing the heat resistance of the polyester resin (1-A).
From such a viewpoint, the mixing ratio of the polyester resin (1-A) and the polyester resin (1-B) is 80:20 or more, particularly 70:30 or more, particularly the polyester resin (1-B). The polyester resin (1-B) is preferably mixed as described above, while the polyester resin (1-B) is contained in a ratio of 40:60 or less, particularly 50:50 or less. -B) is preferably mixed.
第1の難燃性樹脂組成物には、耐加水分解性を付与するためにカルボジイミド化合物を配合してもよい。但し、配合しなくてもよい。 (Other ingredients)
A carbodiimide compound may be blended with the first flame-retardant resin composition in order to impart hydrolysis resistance. However, it is not necessary to mix.
-(N=C=N-R-)n-
(上記式において、nは1以上の整数を示す。Rはその他の有機系結合単位を示す。これらのカルボジイミド化合物は、Rの部分が、脂肪族、脂環族、芳香族のいずれかでもよい。)
通常nは1~50の間で適宜決められる。 Examples of the carbodiimide compound include those having a basic structure represented by the following general formula.
-(N = C = NR-) n-
(In the above formula, n represents an integer of 1 or more. R represents another organic bond unit. In these carbodiimide compounds, the R portion may be aliphatic, alicyclic, or aromatic. .)
Usually, n is appropriately determined between 1 and 50.
かかる観点から、カルボジイミド化合物の配合量は、第1の難燃性樹脂組成物100質量部に対し、0.5質量%以上であるのがさらに好ましく、中でも1質量%以上であるのが特に好ましい。また、4質量%以下であるのがさらに好ましく、中でも3質量%以下であるのが好ましい。 The amount of the carbodiimide compound is preferably 0.1 to 5 parts by mass with respect to 100 parts by mass of the first flame retardant resin composition. By mix | blending a carbodiimide compound in this range, the outstanding hydrolysis resistance can be provided, without reducing heat resistance.
From this point of view, the blending amount of the carbodiimide compound is more preferably 0.5% by mass or more, particularly preferably 1% by mass or more, with respect to 100 parts by mass of the first flame retardant resin composition. . Moreover, it is more preferable that it is 4 mass% or less, and it is preferable that it is 3 mass% or less especially.
第1の難燃性樹脂組成物は、難燃性、柔軟性、機械特性及び耐熱性を備えたものに調製することができる。 より具体的には、難燃性に関しては、Underwriters Laboratories社が規定するUL94垂直燃焼試験において、VTM-0の規格を満たす難燃性を得ることができる。
機械特性に関しては、JIS C 2318に基づいて引張破断強度の測定を行った場合に、引張強度を10MPa以上、好ましくは15MPa以上に調製することができる。
柔軟性に関しては、JIS C 2318に基づいて引張破断伸度の測定を行った場合に、引張伸度を10%以上、好ましくは20%以上に調製することができる。
耐熱性に関しては、JIS K7121に基づいて結晶融解熱量ΔHmの測定を行った場合に、結晶融解熱量(ΔHm)を1J/g以上、好ましくは3J/g以上に調製することができる。 <Physical characteristics of the first flame-retardant resin composition>
The first flame retardant resin composition can be prepared to have flame retardancy, flexibility, mechanical properties, and heat resistance. More specifically, regarding the flame retardancy, flame retardancy satisfying the VTM-0 standard can be obtained in the UL94 vertical combustion test defined by Underwriters Laboratories.
Regarding the mechanical properties, when the tensile strength at break is measured based on JIS C 2318, the tensile strength can be adjusted to 10 MPa or more, preferably 15 MPa or more.
Regarding the flexibility, when the tensile elongation at break is measured according to JIS C 2318, the tensile elongation can be adjusted to 10% or more, preferably 20% or more.
Regarding heat resistance, when the crystal melting heat quantity ΔHm is measured based on JIS K7121, the crystal melting heat quantity (ΔHm) can be adjusted to 1 J / g or more, preferably 3 J / g or more.
第1の難燃性樹脂組成物は、フィルム、シート、プレート或いは射出成形品等の難燃性樹脂体に成形することができる。具体的には、ポリエステル系樹脂(1-A)およびメラミン、必要に応じてポリエステル系樹脂(1-B)などのその他の樹脂や添加物等の原料を直接混合し、押出機或いは射出成型機に投入して成形するか、また、は、前記原料を二軸押出機を用いて溶融混合し、ストランド形状に押出してペレットを作成した後、このペレットを押出機或いは射出成型機に投入して成形する方法を挙げることができる。いずれの方法においても、ポリエステル系樹脂の加水分解による分子量の低下を考慮する必要があり、均一に混合させるためには後者を選択するのが好ましい。そこで、以下後者の製造方法について説明する。 <Use of first flame retardant resin composition>
The first flame retardant resin composition can be formed into a flame retardant resin body such as a film, a sheet, a plate, or an injection molded product. Specifically, raw materials such as polyester resin (1-A) and melamine and, if necessary, other resins and additives such as polyester resin (1-B) are directly mixed, and an extruder or injection molding machine. Or the raw material is melt-mixed using a twin screw extruder, extruded into a strand shape to create a pellet, and then the pellet is put into an extruder or an injection molding machine. A method of molding can be mentioned. In any method, it is necessary to consider a decrease in molecular weight due to hydrolysis of the polyester-based resin, and the latter is preferably selected for uniform mixing. Therefore, the latter manufacturing method will be described below.
この際、ポリエステル系樹脂(1-A)(1-B)の組成比、例えばテレフタル酸の含有割合によって融点が変化すること、及び、各原料の配合割合によって粘度が変化すること等を考慮して、溶融押出温度を適宜選択することが好ましい。また、メラミンの昇華温度も考慮に入れ、成形温度は160℃以上220℃以下、特に210℃未満の温度範囲に調整することが好ましい。 The polyester resin (1-A) and melamine, and if necessary, other resins and additives such as the polyester resin (1-B) are sufficiently dried to remove moisture, and then used with a twin screw extruder. It is melt mixed and extruded into a strand shape to produce pellets.
At this time, considering that the melting point changes depending on the composition ratio of the polyester resins (1-A) and (1-B), for example, the content ratio of terephthalic acid, and that the viscosity changes depending on the mixing ratio of each raw material. Thus, it is preferable to appropriately select the melt extrusion temperature. In consideration of the sublimation temperature of melamine, the molding temperature is preferably adjusted to a temperature range of 160 ° C. or higher and 220 ° C. or lower, particularly less than 210 ° C.
その他目的に合わせて、上記の方法以外でインモールド成形法、ガスプレス成形法、2色成形法、サンドイッチ成形法、PUSH-PULL、SCORIM等を採用することもできる。 The molding method of the injection molded body is not particularly limited, and for example, an injection molding method such as a general injection molding method for a thermoplastic resin, a gas assist molding method, and an injection compression molding method can be employed.
In addition to the above methods, an in-mold molding method, a gas press molding method, a two-color molding method, a sandwich molding method, PUSH-PULL, SCORIM, or the like can also be employed according to other purposes.
この際、難燃剤を含有しない層としては、特に限定するものではなく、例えば耐熱性、機械特性、表面特性を付与する目的の場合には、上記延伸ポリエチレンテレフタレートフィルム等からなる層を形成することが好ましい。また、他の材料との接着性を向上させて粘着テープ等の用途に用いる目的の場合には、ゴム系、アクリル系、ビニルエーテル系等の溶剤型、あるいは、エマルジョン型の粘着剤からなる粘着層を形成するのが好ましい。
この際、積層体の全厚みに占める難燃性ポリエステル系樹脂組成物からなる層の厚みの割合は、20~95%とするのが好ましい。かかる範囲内に難燃性ポリエステル系樹脂組成物の厚み比を設定することにより、難燃性、機械特性を損なうことのない積層体を提供することができる。かかる観点から、積層体の全厚みに占める難燃性ポリエステル系樹脂組成物からなる層の厚みの割合は、30%以上であるのが特に好ましく、中でも40%以上であるのが好ましく、80%以下であるのが特に好ましく、中でも70%以下であるのが好ましい。 Moreover, the laminated body can also be formed by providing one or more layers not containing a flame retardant on one side or both sides of the layer made of the first flame retardant resin composition.
At this time, the layer containing no flame retardant is not particularly limited. For example, in the case of imparting heat resistance, mechanical properties, and surface properties, a layer made of the stretched polyethylene terephthalate film or the like is formed. Is preferred. For the purpose of improving adhesiveness with other materials and using for adhesive tapes, etc., adhesive layer made of rubber, acrylic, vinyl ether or other solvent type or emulsion type adhesives Is preferably formed.
At this time, the ratio of the thickness of the layer made of the flame-retardant polyester resin composition to the total thickness of the laminate is preferably 20 to 95%. By setting the thickness ratio of the flame-retardant polyester resin composition within such a range, it is possible to provide a laminate that does not impair flame retardancy and mechanical properties. From this viewpoint, the ratio of the thickness of the layer composed of the flame-retardant polyester resin composition in the total thickness of the laminate is particularly preferably 30% or more, and particularly preferably 40% or more, and 80%. It is particularly preferable that the ratio is 70% or less.
第2の実施形態に係る難燃性ポリエステル系樹脂組成物(以下「第2の難燃性樹脂組成物」という)について説明する。 [Second Embodiment]
The flame-retardant polyester resin composition according to the second embodiment (hereinafter referred to as “second flame-retardant resin composition”) will be described.
そこで本発明は、第2の実施形態として、ポリエステル系樹脂に難燃化剤としてのメラミンを配合してなる難燃性ポリエステル系樹脂組成物において、成形途中にメラミンが分解して成形不良を生じることがなく、しかも塩化ビニルのような応力緩和特性を備えた、新たな第2の難燃性樹脂組成物難を提案するものである。 Simply adding melamine to a polyester-based resin is inferior in stress relaxation characteristics as compared to a vinyl chloride-based resin. For example, when used as a tape material, it has a problem that it is easily peeled off after winding.
Therefore, as a second embodiment of the present invention, in a flame retardant polyester resin composition obtained by blending melamine as a flame retardant into a polyester resin, the melamine is decomposed during molding, resulting in poor molding. In addition, the present invention proposes a new second flame retardant resin composition difficulty that has no stress and has a stress relaxation property such as vinyl chloride.
このように優れた柔軟性及び機械特性を有する特定のポリエステル系樹脂(2-A)に対してメラミンを配合することで、ポリエステル系樹脂が本来有する特性を損なうことなく、従来検討されてきた無機系難燃剤よりも低添加量で、かつ、優れた難燃性を付与することができる。
また、フェノキシ樹脂は、特定のポリエステル系樹脂(2-A)と完全相溶するため、凝集力のあるフェノキシ樹脂をポリエステル系樹脂中に微分散させることができ、優れた応力緩和特性を得ることができる。しかも、フェノキシ樹脂は、炭化し易い性質を有しているため、フェノキシ樹脂の炭化促進効果とメラミンの燃焼化効果とが相乗的に働き、メラミンの配合量を抑えつつ難燃化をより一層向上させることができる。
以下、詳細に説明する。 Polyester resin containing 50 to 90 mol% terephthalic acid as the polyvalent carboxylic acid component and 70 to 100 mol% in total of 1,4-butanediol, ethylene glycol and diethylene glycol as the polyhydric alcohol component (2-A) has a lower melting point than general polyester resins such as PET and PBT, and can be molded at a temperature lower than the temperature at which melamine decomposes. It is possible to eliminate the occurrence of defects. In addition, excellent flexibility and mechanical properties can be obtained.
By blending melamine with the specific polyester resin (2-A) having such excellent flexibility and mechanical properties, inorganic materials that have been studied in the past without impairing the inherent properties of the polyester resin. The addition amount is lower than that of the system flame retardant, and excellent flame retardancy can be imparted.
Moreover, since the phenoxy resin is completely compatible with the specific polyester resin (2-A), the cohesive phenoxy resin can be finely dispersed in the polyester resin, and excellent stress relaxation characteristics can be obtained. Can do. Moreover, since phenoxy resin has the property of being easily carbonized, the carbonization promoting effect of phenoxy resin and the combustion effect of melamine work synergistically, further improving flame retardancy while suppressing the amount of melamine compounded. Can be made.
Details will be described below.
第2の難燃性樹脂組成物は、ポリエステル系樹脂(2-A)、メラミン、及び、フェノキシ樹脂の混合物を含有する難燃性ポリエステル系樹脂組成物である。 <Composition of the second flame-retardant resin composition>
The second flame retardant resin composition is a flame retardant polyester resin composition containing a mixture of polyester resin (2-A), melamine, and phenoxy resin.
ポリエステル系樹脂(2-A)は、多価カルボン酸と多価アルコールとの重縮合ポリマーであるポリエステル系樹脂(2-A)を主成分とする樹脂組成物であり、当該ポリエステル系樹脂(2-A)は、多価カルボン酸成分として、テレフタル酸を50~90mol%含有し、かつ、多価アルコール成分として、1,4-ブタンジオール、エチレングリコール、及び、ジエチレングリコールを合計で70~100mol含有するポリエステル系樹脂であるのが好ましい。
このような組成を有するポリエステル系樹脂(2-A)を主成分とする樹脂組成物は、PETやPBT等の一般的なポリエステル系樹脂に比べて融点が低く、メラミンが分解する温度よりも低温域で成形可能であるため、成形途中でメラミンが分解して成形不良を生じることを無くすことができる。しかも、優れた柔軟性及び機械特性を得ることができる。
かかる観点から、ポリエステル系樹脂(2-A)は、多価カルボン酸成分として、テレフタル酸を55mol%以上、特に60mol%以上含有するのがさらに好ましく、85mol%以下、特に80mol%以下含有するのがさらに好ましい。また、多価アルコール成分として、1,4-ブタンジオール、エチレングリコール、及び、ジエチレングリコールを合計で75mol%以上、特に80mol%以上含有するのが好ましく、100mol%含有するのがさらに好ましい。
但し、多価アルコール成分としては、1,4-ブタンジオール、エチレングリコール及びジエチレングリコールのうちのいずれか一種を含んでいてもよいし、2種以上を含んでいてもよい。 (Polyester resin (2-A))
The polyester resin (2-A) is a resin composition mainly composed of a polyester resin (2-A) which is a polycondensation polymer of a polyvalent carboxylic acid and a polyhydric alcohol. -A) contains 50 to 90 mol% of terephthalic acid as the polyvalent carboxylic acid component, and 70 to 100 mol in total of 1,4-butanediol, ethylene glycol, and diethylene glycol as the polyhydric alcohol component It is preferable to use a polyester resin.
The resin composition mainly composed of the polyester resin (2-A) having such a composition has a melting point lower than that of general polyester resins such as PET and PBT, and is lower than the temperature at which melamine decomposes. Since molding is possible in the region, it is possible to eliminate the occurrence of molding defects due to decomposition of melamine during molding. In addition, excellent flexibility and mechanical properties can be obtained.
From this point of view, the polyester resin (2-A) preferably contains terephthalic acid as a polyvalent carboxylic acid component in an amount of 55 mol% or more, particularly 60 mol% or more, more preferably 85 mol% or less, particularly 80 mol% or less. Is more preferable. Further, as the polyhydric alcohol component, 1,4-butanediol, ethylene glycol and diethylene glycol are contained in a total amount of 75 mol% or more, particularly preferably 80 mol% or more, and more preferably 100 mol%.
However, the polyhydric alcohol component may include any one of 1,4-butanediol, ethylene glycol, and diethylene glycol, or may include two or more.
ポリエステル系樹脂(a-1)(a-2)の混合物をポリエステル系樹脂(2-A)の主成分として用いることにより、優れた機械特性、柔軟性を兼ね備えた樹脂組成物を提供することができる。特にポリエステル系樹脂(a-2)を配合することによって、柔軟性、特に伸び易さを高めることができる。 The polyester resin (2-A) may be a polyester resin mainly composed of a mixture of two or more polyester resins. Among them, a polyester resin containing isophthalic acid in a ratio of 5 mol% or more and less than 30 mol% in the polyvalent carboxylic acid component and ethylene glycol in a ratio of 0 mol% or more and less than 50 mol% in the polyhydric alcohol component ( a-1), the polycarboxylic acid component contains isophthalic acid in a proportion of 30 mol% to 50 mol%, and the polyhydric alcohol component contains ethylene glycol in a proportion of 50 mol% to 100 mol%. A mixture with the polyester resin (a-2) is a particularly preferred example.
By using a mixture of polyester resins (a-1) and (a-2) as a main component of polyester resin (2-A), a resin composition having excellent mechanical properties and flexibility can be provided. it can. In particular, by blending the polyester resin (a-2), flexibility, particularly ease of elongation, can be enhanced.
また、ポリエステル系樹脂(a-1)における多価アルコール成分中のエチレングリコールの含有割合は、5mol%以上、特に10mol%以上であるのがさらに好ましく、45mol%未満、特に40mol%未満であるのがさらに好ましい。 At this time, the content ratio of isophthalic acid in the polyvalent carboxylic acid component in the polyester resin (a-1) is more preferably 7 mol% or more, particularly preferably 10 mol% or more, less than 25 mol%, particularly less than 20 mol%. More preferably.
Further, the content ratio of ethylene glycol in the polyhydric alcohol component in the polyester resin (a-1) is more preferably 5 mol% or more, particularly preferably 10 mol% or more, and less than 45 mol%, particularly less than 40 mol%. Is more preferable.
また、ポリエステル系樹脂(a-2)における多価アルコール成分中のエチレングリコールの含有割合は、55mol%以上、特に60mol%以上であるのがさらに好ましく、90mol%以下、特に80mol%以下であるのがさらに好ましい。 The content ratio of isophthalic acid in the polyvalent carboxylic acid component in the polyester-based resin (a-2) is more preferably 33 mol% or more, particularly 35 mol% or more, and more preferably 43 mol% or less, particularly 40 mol% or less. Further preferred.
Further, the content ratio of ethylene glycol in the polyhydric alcohol component in the polyester resin (a-2) is more preferably 55 mol% or more, particularly preferably 60 mol% or more, and 90 mol% or less, particularly 80 mol% or less. Is more preferable.
かかる観点から、ポリエステル系樹脂(2-A)の質量平均分子量は、特に20,000以上、中でも特に30,000以上であるのがさらに好ましく、特に200,000以下、中でも特に150,000以下であるのがさらに好ましい。 The mass average molecular weight of the polyester resin (2-A) (in the case of two types, the average thereof) is preferably 10,000 to 300,000. If the mass average molecular weight of the polyester-based resin (2-A) is within such a range, flexibility can be obtained, and the melt viscosity is appropriate, so that there is little possibility of problems in molding.
From this viewpoint, the mass average molecular weight of the polyester-based resin (2-A) is particularly preferably 20,000 or more, more preferably 30,000 or more, particularly 200,000 or less, especially 150,000 or less. More preferably.
ゲルパーミエーションクロマトグラフィーを用いて、溶媒クロロホルム、溶液濃度0.2wt/vol%、溶液注入量200μL、溶媒流速1.0ml/分、溶媒温度40℃で測定を行い、ポリスチレン換算で質量平均分子量を算出することができる。この際に用いる標準ポリスチレンの質量平均分子量は、2000000、430000、110000、35000、10000、4000、600である。 The mass average molecular weight can be measured by the following method. The same applies to other resins.
Using gel permeation chromatography, measurement is made at a solvent chloroform, a solution concentration of 0.2 wt / vol%, a solution injection amount of 200 μL, a solvent flow rate of 1.0 ml / min, a solvent temperature of 40 ° C., and a mass average molecular weight in terms of polystyrene is obtained. Can be calculated. The mass average molecular weight of the standard polystyrene used in this case is 20000, 430000, 110000, 35000, 10000, 4000, 600.
メラミンは、第1の難燃性樹脂組成物に用いるメラミンと同様であり、同様の作用を得ることができる。また、第1の難燃性樹脂組成物と同様に、本発明の効果を損なわない範囲で、メラミンと他の難燃剤ないし難燃助剤を併用しても構わない。 (melamine)
Melamine is similar to the melamine used in the first flame retardant resin composition, and can obtain the same action. Similarly to the first flame retardant resin composition, melamine and other flame retardants or flame retardant aids may be used in combination as long as the effects of the present invention are not impaired.
フェノキシ樹脂は、ビスフェノールAなどの芳香族二価フェノール系化合物とエピクロルヒドリンとの反応で得られる樹脂である。
フェノキシ樹脂は、特定のポリエステル系樹脂(2-A)と完全相溶するため、凝集力のあるフェノキシ樹脂をポリエステル系樹脂(2-A)中に微分散させることができ、その結果、優れた応力緩和特性を得ることができる。しかも、フェノキシ樹脂は、炭化し易い性質を有しているため、メラミンの燃焼化効果と相乗的に働き、メラミンの配合量を抑えつつ第2の難燃性樹脂組成物の難燃化をより一層向上させることができる。 (Phenoxy resin)
The phenoxy resin is a resin obtained by a reaction between an aromatic dihydric phenol compound such as bisphenol A and epichlorohydrin.
Since the phenoxy resin is completely compatible with the specific polyester resin (2-A), the cohesive phenoxy resin can be finely dispersed in the polyester resin (2-A). Stress relaxation characteristics can be obtained. Moreover, since the phenoxy resin has the property of being easily carbonized, it works synergistically with the combustion effect of melamine, reducing the amount of melamine added and reducing the flame retardancy of the second flame retardant resin composition. This can be further improved.
第2の難燃性樹脂組成物中に占めるメラミンの配合割合は、10~60質量%であるのが好ましい。第2の難燃性樹脂組成物中に占めるメラミンの配合割合が10質量%以上であれば、十分な難燃性を得ることができる一方、メラミンの配合割合が60質量%以下であれば機械物性を損なうことがない。かかる観点から、第2の難燃性樹脂組成物中に占めるメラミンの配合割合は、20質量%以上であるのが特に好ましく、中でも30質量%以上であるのがさらに好ましい。また、50質量%以下であるのが特に好ましく、中でも40質量%以下であるのがさらに好ましい。 (Mixing ratio)
The blending ratio of melamine in the second flame retardant resin composition is preferably 10 to 60% by mass. If the blending ratio of melamine in the second flame-retardant resin composition is 10% by mass or more, sufficient flame retardancy can be obtained, while if the blending ratio of melamine is 60% by mass or less, the machine There is no loss of physical properties. From such a viewpoint, the blending ratio of melamine in the second flame retardant resin composition is particularly preferably 20% by mass or more, and more preferably 30% by mass or more. Moreover, it is especially preferable that it is 50 mass% or less, and it is still more preferable that it is 40 mass% or less especially.
特に、第2の難燃性樹脂組成物からテープを作成する場合には、フェノキシ樹脂を配合することによって、ポリエステル系樹脂(2-A)のガラス転移温度Tgを40~50℃に調整するのが好ましい。 The blending ratio of the phenoxy resin in the second flame retardant resin composition is preferably 1 to 25% by mass. When the blending ratio of the phenoxy resin is within such a range, stress relaxation characteristics and flame retardancy can be improved. From this viewpoint, the ratio of the phenoxy resin in the second flame retardant resin composition is preferably 2% by mass or more, and more preferably 5% by mass or more. Moreover, it is preferable that it is 20 mass% or less, and it is still more preferable that it is 10 mass% or less especially.
In particular, when a tape is prepared from the second flame retardant resin composition, the glass transition temperature Tg of the polyester resin (2-A) is adjusted to 40 to 50 ° C. by blending the phenoxy resin. Is preferred.
第2の難燃性樹脂組成物には、耐加水分解性を付与するためにカルボジイミド化合物を配合してもよい。但し、配合しなくてもよい。
配合するカルボジイミド化合物の種類及び配合量は、第1の難燃性樹脂組成物において説明した配合するカルボジイミド化合物と同様である。 (Other ingredients)
A carbodiimide compound may be blended with the second flame retardant resin composition in order to impart hydrolysis resistance. However, it is not necessary to mix.
The kind and the compounding quantity of the carbodiimide compound to mix | blend are the same as the carbodiimide compound to mix | blend demonstrated in the 1st flame-retardant resin composition.
第2の難燃性樹脂組成物は、難燃性、柔軟性、機械特性及び応力緩和特性を備えることができ、さらに耐熱性を備えたものに調製することができる。
より具体的には、難燃性に関しては、Underwriters Laboratories社が規定するUL94垂直燃焼試験において、VTM-0の規格を満たす難燃性を得ることができる。
機械特性に関しては、JIS C 2318に基づいて引張破断強度の測定を行った場合に、引張強度を10MPa以上、好ましくは15MPa以上に調製することができる。
柔軟性に関しては、JIS C 2318に基づいて引張破断伸度の測定を行った場合に、引張伸度を10%以上、好ましくは20%以上に調製することができる。
応力緩和特性に関しては、JIS C 2318に基づいて応力緩和率を測定した場合に、応力緩和率を50%以上、好ましくは55%以上に調製することができる。
耐熱性に関しては、JIS K7121に基づいて結晶融解熱量ΔHmの測定を行った場合に、結晶融解熱量(ΔHm)を1J/g以上、好ましくは5J/g以上に調製することができる。 <Physical characteristics of second flame retardant resin composition>
The second flame retardant resin composition can have flame retardancy, flexibility, mechanical properties, and stress relaxation properties, and can be further prepared with heat resistance.
More specifically, regarding the flame retardancy, flame retardancy satisfying the VTM-0 standard can be obtained in the UL94 vertical combustion test defined by Underwriters Laboratories.
Regarding the mechanical properties, when the tensile strength at break is measured based on JIS C 2318, the tensile strength can be adjusted to 10 MPa or more, preferably 15 MPa or more.
Regarding the flexibility, when the tensile elongation at break is measured according to JIS C 2318, the tensile elongation can be adjusted to 10% or more, preferably 20% or more.
Regarding the stress relaxation characteristics, when the stress relaxation rate is measured based on JIS C 2318, the stress relaxation rate can be adjusted to 50% or more, preferably 55% or more.
Regarding heat resistance, when the crystal melting heat quantity ΔHm is measured based on JIS K7121, the crystal melting heat quantity (ΔHm) can be adjusted to 1 J / g or more, preferably 5 J / g or more.
第2の難燃性樹脂組成物は、フィルム、シート、プレート或いは射出成形品等の難燃性樹脂体に成形することができる。その際の具体的な成形方法は、第1の難燃性樹脂組成物と同様である。 <Use of second flame retardant resin composition>
The second flame retardant resin composition can be formed into a flame retardant resin body such as a film, a sheet, a plate, or an injection molded product. The specific molding method at that time is the same as that of the first flame-retardant resin composition.
中でも、第2の難燃性樹脂組成物は、優れた応力緩和特性を備えているため、所謂ビニルテープの代替材料、特に難燃性ビニルテープの代替材料として特に優れている。 The second flame retardant resin composition has excellent flame retardancy, mechanical properties, and flexibility, so that it can be used for cellular phone parts, cable coating materials, packings, films and sheets for electrical insulation, and flat cable materials. It can be widely used for household appliances such as vibration damping materials, and for fields such as adhesive tape base materials, rolls, water shielding sheets, gaskets, anti-slip materials, wire clothing materials, and other building materials and industrial applications. In addition, since it does not contain a halogen compound or a phosphorus compound, it is possible to provide a material with excellent safety that does not cause problems such as environmental pollution.
Among these, since the second flame retardant resin composition has excellent stress relaxation properties, the second flame retardant resin composition is particularly excellent as a substitute material for a so-called vinyl tape, particularly as a substitute material for the flame retardant vinyl tape.
次に、第3の実施形態に係る難燃性積層体(「第3の難燃性積層体」と称する)について説明する。 [Third Embodiment]
Next, a flame retardant laminate (referred to as “third flame retardant laminate”) according to a third embodiment will be described.
ここで、「1表面上に」とは、A層表面上に、直にB層を設ける場合、及びA層表面上に単層また、は多層である他の層を設け、前記他の層上にB層を設けることを意味するものである。
第3の難燃性積層体によれば、特定のポリエステル樹脂を使用しており、A層は優れた難燃性を有するため、特に難燃剤を含有しないB層を片側また、は両側に積層した場合においても、積層体全体として優れた難燃性を発現することが可能である。
また、本発明によればハロゲン系化合物、およびリン化合物を含有しないため、環境汚染等の問題を引き起こすことのない安全性に優れた材料を提供することができる。 The third flame retardant laminate has an A and a main component of a mixture of a polyester resin (3-A) having a glass transition temperature of 30 ° C. or less and a heat of crystal fusion ΔHm of 40 J / g or less and melamine. A flame retardant laminate having a B layer on at least one surface of the layer, wherein the content of melamine in the total mass of the A layer is 10 to 80% by mass.
Here, “on one surface” means that the B layer is provided directly on the surface of the A layer, and that another layer that is a single layer or a multilayer is provided on the surface of the A layer. This means that the B layer is provided on the top.
According to the third flame retardant laminate, since a specific polyester resin is used and the A layer has excellent flame retardancy, the B layer not containing a flame retardant is particularly laminated on one side or both sides. Even in this case, it is possible to exhibit excellent flame retardancy as a whole laminate.
In addition, according to the present invention, since a halogen-based compound and a phosphorus compound are not contained, it is possible to provide a material having excellent safety without causing problems such as environmental pollution.
第3の難燃性積層体のA層は、主にポリエステル系樹脂(3-A)とメラミンから構成される層である。 <A layer>
The A layer of the third flame retardant laminate is a layer mainly composed of a polyester resin (3-A) and melamine.
第3の難燃性積層体で使用されるポリエステル系樹脂(3-A)は、ガラス転移温度が30℃以下であり、かつ結晶融解熱量ΔHmが40J/g以下であることが重要である。この条件を満たすことにより、ポリエステル系樹脂(3-B)との接着性が良好であり、2次加工、及び、使用時における層間での剥離を生じることのない積層体を提供することができる。また、第3の難燃性積層体におけるポリエステル系樹脂(3-A)は、単一の樹脂であっても、二種類以上の樹脂の混合物であってもよい。ポリエステル系樹脂(3-A)の具体例としては、多価カルボン酸と多価アルコールを重合して得られる芳香族ポリエステル乳酸系樹脂等の脂肪族ポリエステルが挙げられる。 (Polyester resin (3-A))
It is important that the polyester resin (3-A) used in the third flame-retardant laminate has a glass transition temperature of 30 ° C. or lower and a crystal melting heat ΔHm of 40 J / g or lower. By satisfying this condition, it is possible to provide a laminate that has good adhesion to the polyester resin (3-B) and does not cause separation between layers during secondary processing and use. . Further, the polyester resin (3-A) in the third flame-retardant laminate may be a single resin or a mixture of two or more kinds of resins. Specific examples of the polyester resin (3-A) include aliphatic polyesters such as aromatic polyester lactic acid resins obtained by polymerizing polyvalent carboxylic acids and polyhydric alcohols.
なお、第3の難燃性積層体に用いるポリエステル系樹脂(3-A)のガラス転移温度の下限値、及び結晶融解熱量ΔHmの下限値は特に限定されるものではないが、前記ガラス転移温度が-100℃以上であり、結晶融解熱量ΔHmが0J/g以上であれば、全ての実用温度域において、ポリエステル系樹脂(3-B)との優れた接着強度が得られる。 The glass transition temperature of the polyester resin (3-A) used for the third flame retardant laminate is 30 ° C. or lower, preferably 20 ° C. or lower, more preferably 10 ° C. or lower. In addition, the heat of crystal fusion ΔHm of the polyester resin (3-A) used for the third flame retardant laminate is 40 J / g or less, preferably 25 J / g or less, and more preferably 20 J / g or less. If the glass transition temperature of the polyester resin (3-A) is 30 ° C. or less and the heat of crystal fusion ΔHm is 40 J / g or less, the polyester resin (3- The problem of peeling with B) does not occur.
The lower limit value of the glass transition temperature of the polyester resin (3-A) used in the third flame-retardant laminate and the lower limit value of the crystal melting heat amount ΔHm are not particularly limited, but the glass transition temperature is not limited. Is -100 ° C. or higher, and the heat of crystal fusion ΔHm is 0 J / g or higher, excellent adhesive strength with the polyester resin (3-B) can be obtained in all practical temperature ranges.
メラミンは、第1の難燃性樹脂組成物に用いるメラミンと同様であり、同様の作用を得ることができる。また、第1の難燃性樹脂組成物と同様に、第3の難燃性積層体の効果を損なわない範囲で、メラミンと他の難燃剤ないし難燃助剤を併用しても構わない。 (melamine)
Melamine is similar to the melamine used in the first flame retardant resin composition, and can obtain the same action. Similarly to the first flame retardant resin composition, melamine and other flame retardants or flame retardant aids may be used in combination as long as the effects of the third flame retardant laminate are not impaired.
第3の難燃性積層体のA層は、ポリエステル系樹脂Aとメラミンとの混合物を主成分としている。
ポリエステル系樹脂Aとメラミンとの混合物は、前記した配合割合により構成され、単軸また、は2軸押出機により、押出すことにより混合物を作製し、A層を形成する。 (blend)
The A layer of the third flame retardant laminate is mainly composed of a mixture of polyester resin A and melamine.
The mixture of the polyester resin A and melamine is constituted by the above-described blending ratio, and the mixture is produced by extrusion with a single screw or twin screw extruder to form the A layer.
第3の難燃性積層体を構成するB層は、特に限定されず、公知の層を構成することが可能な材料を使用することが可能である。例えば、熱可塑性樹脂、金属等が挙げられる。
但し、耐熱性、機械特性、表面特性を付与する目的であれば、ポリエステル系樹脂(3-B)を用いることが好ましい。また、さらに他の材料との接着性を向上し、粘着テープ等の用途へ用いる目的であれば、ゴム系、アクリル系、ビニルエーテル系等の溶剤型、あるいは、エマルジョン型の粘着剤を用いることが好ましい。
以下、詳細に説明する。 <B layer>
B layer which comprises a 3rd flame-retardant laminated body is not specifically limited, It is possible to use the material which can comprise a well-known layer. For example, a thermoplastic resin, a metal, etc. are mentioned.
However, for the purpose of imparting heat resistance, mechanical properties, and surface properties, it is preferable to use a polyester resin (3-B). In addition, if the purpose is to improve the adhesion to other materials and use it for applications such as pressure-sensitive adhesive tapes, it is possible to use rubber-type, acrylic-type, vinyl ether-type solvent-type or emulsion-type pressure-sensitive adhesives. preferable.
Details will be described below.
第3の難燃性積層体に用いるポリエステル系樹脂(3-B)としては、ガラス転移温度が50℃以上、かつ、結晶融解熱量ΔHmが40J/g以上であることが好ましい。この条件を満たすことにより、優れた耐熱性を有する積層体を提供することができる。ポリエステル系樹脂(3-B)の具体例としては、多価カルボン酸と多価アルコールを重合して得られる芳香族ポリエステル、乳酸系樹脂等の脂肪族ポリエステルが挙げられる。 (Polyester resin (3-B))
The polyester resin (3-B) used for the third flame retardant laminate preferably has a glass transition temperature of 50 ° C. or higher and a crystal melting heat ΔHm of 40 J / g or higher. By satisfying this condition, a laminate having excellent heat resistance can be provided. Specific examples of the polyester resin (3-B) include aliphatic polyesters such as aromatic polyesters and lactic acid resins obtained by polymerizing polyvalent carboxylic acids and polyhydric alcohols.
なお、第3の難燃性積層体に用いるポリエステル系樹脂(3-B)のガラス転移温度の下限値、及び結晶融解熱量ΔHmの上限値は特に限定されるものではないが、前記ガラス転移温度が100℃以下であり、結晶融解熱量ΔHmが90J/g以下であれば、十分な耐熱性を備えた積層体が得られる。 The glass transition temperature of the polyester resin (3-B) used for the third flame-retardant laminate is 50 ° C. or higher, preferably 55 ° C. or higher, and more preferably 60 ° C. or higher. In addition, the heat of crystal fusion ΔHm of the polyester resin (3-B) used for the third flame-retardant laminate is 40 J / g or more, preferably 45 J / g or more, and more preferably 50 J / g or more. If the glass transition temperature of the polyester resin (3-A) is 50 ° C. or more and the heat of crystal fusion ΔHm is 40 J / g or more, there is a problem of insufficient heat resistance during secondary processing and use. Does not occur.
The lower limit value of the glass transition temperature of the polyester resin (3-B) used in the third flame retardant laminate and the upper limit value of the heat of crystal fusion ΔHm are not particularly limited, but the glass transition temperature is not limited. Is 100 ° C. or less, and the crystal melting heat ΔHm is 90 J / g or less, a laminate having sufficient heat resistance can be obtained.
第3の難燃性積層体にさらに耐加水分解性を付与するために、カルボジイミド化合物を配合することができる。但し、配合しなくてもよい。
配合するカルボジイミド化合物の種類は、第1の難燃性樹脂組成物において説明した配合するカルボジイミド化合物と同様である。 (Carbodiimide compound)
In order to further impart hydrolysis resistance to the third flame retardant laminate, a carbodiimide compound can be blended. However, it is not necessary to mix.
The kind of carbodiimide compound to mix | blend is the same as the carbodiimide compound to mix | blend demonstrated in the 1st flame retardant resin composition.
第3の難燃性積層体のA層、B層間の剥離強度は、23℃で通常3N/cm以上であり、好ましくは4N/cm以上、より好ましくは5N/cm以上である。A層とB層が3N/cm以上であれば積層体として、一体として様々な用途に使用可能である。 <Physical characteristics of the third flame retardant laminate>
The peel strength between the A layer and the B layer of the third flame retardant laminate is usually 3 N / cm or more at 23 ° C., preferably 4 N / cm or more, more preferably 5 N / cm or more. If the A layer and the B layer are 3 N / cm or more, the laminate can be used for various purposes as a unit.
次に、第3の難燃性積層体の製造方法について説明する。
ここでは、フィルム乃至シート状の第3の難燃性積層体の製造方法について説明するが、次に説明する例に限定されるものではない。 <Method for producing third flame-retardant laminate>
Next, the manufacturing method of a 3rd flame-retardant laminated body is demonstrated.
Here, although the manufacturing method of a film thru | or sheet-like 3rd flame-retardant laminated body is demonstrated, it is not limited to the example demonstrated below.
次いで、A層となるフィルム及びB層となるフィルムを加熱するか、或いは、層間に接着層を配置するかして、両者をラミネートすることで第3の難燃性積層体を成形することができる。第3の難燃性積層体の延伸については、共押出の場合と同様である。 In the case of thermal lamination and dry lamination, the raw material constituting the A layer is mixed and kneaded to prepare the resin composition a, and the resin composition a is T-die, I-die, etc. with a single screw or twin screw extruder The resin composition b is prepared by mixing and kneading the raw materials constituting the B layer, and the resin composition b is formed into a T-die by a single screw or twin screw extruder. Extrude from an I die or the like to obtain a film to be a B layer.
Next, the film to be the A layer and the film to be the B layer are heated, or an adhesive layer is disposed between the layers, and the third flame-retardant laminate can be formed by laminating them. it can. The stretching of the third flame retardant laminate is the same as in the case of coextrusion.
アンカーコート層に用いるアンカーコート用接着剤としては、ポリエステル系、ポリウレタン系、アクリル系、PVC-酢酸ビニル共重合体系等の接着剤が挙げられる。また、アンカーコート用接着剤の塗布にはロールコート法、グラビアコート法等を用いることができる。なお、アンカーコート層の厚みは適宜調整することができるが、難燃性、接着性の点から0.1μm~5μmの範囲とすることが好ましい。 In order to further improve the adhesion between the A layer and the B layer, the surface of the B layer on the A layer side may be subjected to a corona discharge treatment, or an anchor coat layer may be provided on the B layer.
Examples of the anchor coat adhesive used for the anchor coat layer include polyester, polyurethane, acrylic, and PVC-vinyl acetate copolymer systems. Moreover, a roll coat method, a gravure coat method, etc. can be used for application | coating of the adhesive agent for anchor coats. The thickness of the anchor coat layer can be appropriately adjusted, but is preferably in the range of 0.1 μm to 5 μm from the viewpoint of flame retardancy and adhesiveness.
第3の難燃性積層体は、優れた難燃性、機械特性、表面特性を兼ね備えているため、電気絶縁材、メンブレンスイッチ回路印刷基材、複写機内部部材、面状発熱体基材、FPC補強板等の用途に用いることができる。 <Use of third flame retardant laminate>
Since the third flame-retardant laminate has excellent flame retardancy, mechanical properties, and surface properties, an electrical insulating material, a membrane switch circuit printing base material, a copier internal member, a planar heating element base material, It can be used for applications such as FPC reinforcing plates.
次に、第4の実施形態に係る難燃性積層体(以下「第4の難燃性積層体」という)について説明する。 [Fourth flame retardant laminate]
Next, a flame retardant laminate according to a fourth embodiment (hereinafter referred to as “fourth flame retardant laminate”) will be described.
そこで本発明は、このような従来技術の課題に鑑み、ハロゲン系化合物およびリン系化合物を含有せずに、金属接着性および難燃性を兼ね備えた新たな金属接着用難燃性樹脂積層体を提供せんとするものである。
すなわち本発明は、第4の難燃性積層体として、金属接着性と難燃性とを兼ね備えた金属接着用難燃性樹脂積層体であって、ガラス転移温度が-80~30℃であるポリエステル系樹脂(4-A)、メラミン、及び、フェノキシ樹脂の混合物を主成分とする樹脂組成物aからなるA層を有し、当該A層上に、ガラス転移温度が50~120℃であり、結晶融解熱量ΔHmが40~100J/gであるポリエステル系樹脂(4-B)を主成分とする樹脂組成物bからなるB層を有する樹脂積層体であり、A層を構成する樹脂組成物a中に占めるメラミンの割合が20~80質量%であり、かつ、樹脂組成物a中に占めるフェノキシ樹脂の割合が1~30質量%であることを特徴とする金属接着用難燃性樹脂積層体を提案するものである。 In the prior art, in order to obtain a high level of flame retardancy that passes VTM-0 in the UL94 vertical combustion test, it is necessary to add a large amount of flame retardant to the adhesive layer. There existed problems, such as adhesiveness with a metal falling. Moreover, when it was going to reduce the quantity of the flame retardant mix | blended with an adhesive bond layer, it was necessary to contain a flame retardant in layers other than an adhesive layer.
Therefore, in view of such problems of the conventional technology, the present invention provides a new metal-bonding flame-retardant resin laminate having both metal adhesion and flame retardancy without containing a halogen compound and a phosphorus compound. It is to be provided.
That is, the present invention is a flame retardant resin laminate for metal adhesion that has both metal adhesion and flame retardancy as a fourth flame retardant laminate, and has a glass transition temperature of −80 to 30 ° C. It has an A layer composed of a resin composition a composed mainly of a mixture of polyester resin (4-A), melamine and phenoxy resin, and has a glass transition temperature of 50 to 120 ° C. on the A layer. A resin laminate having a B layer composed of a resin composition b mainly composed of a polyester resin (4-B) having a crystal melting heat ΔHm of 40 to 100 J / g, and constituting the A layer a flame retardant resin laminate for metal bonding, wherein the proportion of melamine in a is 20 to 80% by mass and the proportion of phenoxy resin in the resin composition a is 1 to 30% by mass The body is proposed.
フェノキシ樹脂は、金属表面に存在する水分と水素結合するため金属との接着性に優れているばかりか、ポリエステル系樹脂と相溶性を有するため、ポリエステル系樹脂(4-A)にフェノキシ樹脂を配合することで、難燃性を低下させることなく、金属との接着性を高めることができる。
また、メラミンは、燃焼時に不燃性のガスを発生するため、接着層を難燃化することができるばかりか、難燃剤を配合してない外層(B層)をも難燃化することができるため、積層体全体の難燃性を格別に高めることができる。
しかも、フェノキシ樹脂とメラミンとを組み合わせてポリエステル系樹脂(4-A)に配合することで、互いの特性を打ち消すことなく、相乗的な効果を得ることができる。 According to the fourth flame-retardant laminate, the specific polyester resin constituting the adhesive layer (A layer) mainly improves the adhesion between melamine for improving flame retardancy and mainly metal. By blending with the phenoxy resin for the purpose, the flame retardancy can be increased, and the adhesiveness between the adhesive layer (A layer) and the metal can be significantly increased. In addition, since it does not contain a halogen compound and a phosphorus compound, it is possible to provide a material with excellent safety that does not cause problems such as environmental pollution.
Phenoxy resin not only has excellent adhesion to metal because it forms hydrogen bonds with moisture present on the metal surface, but also has compatibility with polyester resin, so phenoxy resin is blended with polyester resin (4-A). By doing so, adhesiveness with a metal can be improved, without reducing a flame retardance.
Moreover, since melamine generates a nonflammable gas at the time of combustion, not only the adhesive layer can be made flame retardant, but also the outer layer (B layer) not containing a flame retardant can be made flame retardant. Therefore, the flame retardance of the entire laminate can be particularly enhanced.
In addition, by combining phenoxy resin and melamine in the polyester resin (4-A), a synergistic effect can be obtained without canceling each other's characteristics.
ここで、「A層上に」とは、A層上に直にB層を積層する場合のほか、A層上に他の層を介してB層を積層する場合を包含する意である。 Now, the fourth flame retardant laminate has a polyester resin (4-B) formed on a layer A composed of a resin composition a whose main component is a mixture of polyester resin (4-A), melamine and phenoxy resin. It is a laminated body provided with the B layer which consists of the resin composition b which has as a main component.
Here, “on the A layer” means not only the case where the B layer is laminated directly on the A layer, but also the case where the B layer is laminated on the A layer via another layer.
第4の難燃性積層体においてA層は、接着層の役割を備えた層であり、このA層は、ポリエステル系樹脂(4-A)、メラミン及びフェノキシ樹脂からなる混合物を主成分とする樹脂組成物aからなる層である。 <A layer>
In the fourth flame retardant laminate, the A layer is a layer having a role of an adhesive layer, and this A layer is mainly composed of a mixture of the polyester resin (4-A), melamine and phenoxy resin. It is a layer made of the resin composition a.
ポリエステル系樹脂(4-A)は、ガラス転移温度が-80℃~30℃である樹脂であることが重要である。ポリエステル系樹脂(4-A)のガラス転移温度が-80℃~30℃であれば、低温から通常の使用温度までの広範囲において、優れた機械特性を有する積層体とすることができる。
かかる観点から、ポリエステル系樹脂(4-A)のガラス転移温度は、-70℃以上であるのが特に好ましく、中でも-60℃以上であるのがさらに好ましい。また、20℃以下であるのが特に好ましく、中でも10℃以下であるのがさらに好ましい。 (Polyester resin (4-A))
It is important that the polyester resin (4-A) is a resin having a glass transition temperature of −80 ° C. to 30 ° C. If the glass transition temperature of the polyester resin (4-A) is −80 ° C. to 30 ° C., a laminate having excellent mechanical properties can be obtained in a wide range from a low temperature to a normal use temperature.
From this point of view, the glass transition temperature of the polyester resin (4-A) is particularly preferably −70 ° C. or higher, and more preferably −60 ° C. or higher. Moreover, it is especially preferable that it is 20 degrees C or less, and it is still more preferable that it is 10 degrees C or less especially.
かかる観点から、ポリエステル系樹脂(4-A)の結晶融解熱量ΔHmは特に8J/g以上であるのが好ましく、中でも10J/g以上であるのがさらに好ましい。また、特に25J/g以下であるのが好ましく、中でも20J/g以下であるのがさらに好ましい。 The polyester resin (4-A) is preferably a resin having a heat of crystal fusion ΔHm of 5 to 30 J / g. When the heat of crystal melting ΔHm of the polyester resin (4-A) is 5 to 30 J / g, a laminate having sufficient adhesiveness and heat resistance at the time of molding, secondary processing and use, can do.
From this viewpoint, the heat of crystal fusion ΔHm of the polyester resin (4-A) is particularly preferably 8 J / g or more, and more preferably 10 J / g or more. In particular, it is preferably 25 J / g or less, more preferably 20 J / g or less.
コハク酸、アジピン酸、セバシン酸、アゼライン酸、ドデカン二酸、1,3-シクロヘキサンジカルボン酸および1,4-シクロヘキサンジカルボン酸のうちの1種又は2種以上の脂肪族ジカルボン酸と、
ジエチレングリコール、エチレングリコール、1,2-プロピレングリコール、1,3-プロパンジオール、2,2-ジメチル-1,3-プロパンジオール、トランス-テトラメチル-1,3-シクロブタンジオール、2,2,4,4-テトラメチル-1,3-シクロブタンジオール、1,4-ブタンジオール、ネオペンチルグリコール、1,5-ペンタンジオール、1,6-ヘキサンジオール、1,4-シクロヘキサンジメタノール、1,3-シクロヘキサンジメタノー、デカメチレングリコール、シクロヘキサンジオール、p-キシレンジオール、ビスフェノールA、テトラブロモビスフェノールAおよびテトラブロモビスフェノールA-ビス(2-ヒドロキシエチルエーテル)のうちの1種又は2種以上の多価アルコールと、からなる共重合ポリエステルを挙げることができる。 The aromatic aliphatic polyester used as the polyester resin (4-A) includes terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2,5-dichloroterephthalic acid, 2-methylterephthalic acid, 4,4-stilbene dicarboxylic acid Acid, 4,4-biphenyldicarboxylic acid, orthophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, bisbenzoic acid, bis (p-carboxyphenyl) methane, anthracene dicarboxylic acid, 4,4- One or more aromatic dicarboxylic acids of diphenyl ether dicarboxylic acid, 4,4-diphenoxyethane dicarboxylic acid, 5-Na sulfoisophthalic acid and ethylene-bis-p-benzoic acid;
One or more aliphatic dicarboxylic acids of succinic acid, adipic acid, sebacic acid, azelaic acid, dodecanedioic acid, 1,3-cyclohexanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid;
Diethylene glycol, ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 2,2-dimethyl-1,3-propanediol, trans-tetramethyl-1,3-cyclobutanediol, 2,2,4, 4-tetramethyl-1,3-cyclobutanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, 1,3-cyclohexane One or more polyhydric alcohols of dimethanol, decamethylene glycol, cyclohexanediol, p-xylenediol, bisphenol A, tetrabromobisphenol A and tetrabromobisphenol A-bis (2-hydroxyethyl ether); A copolymer consisting of Riesuteru can be mentioned.
かかる観点から、脂肪族ポリエステルおよび芳香族脂肪族ポリエステルの質量平均分子量は、80,000以上であるのが特に好ましく、中でも100,000以上であるのがさらに好ましい。また、300,000以下であるのが特に好ましく、中でも250,000以下であるのがさらに好ましい。 These aliphatic polyesters and aromatic aliphatic polyesters preferably have a mass average molecular weight of 50,000 to 400,000. If the mass average molecular weight of these polyesters is 50,000 or more, there is no problem that the laminate is damaged due to insufficient flame retardancy or insufficient mechanical strength. Moreover, if a mass average molecular weight is 400,000 or less, the problem of the shaping | molding defect by the viscosity of resin being too high will not generate | occur | produce.
From this viewpoint, the weight average molecular weight of the aliphatic polyester and the aromatic aliphatic polyester is particularly preferably 80,000 or more, and more preferably 100,000 or more. Also, it is particularly preferably 300,000 or less, and more preferably 250,000 or less.
ゲルパーミエーションクロマトグラフィーを用いて、溶媒クロロホルム、溶液濃度0.2wt/vol%、溶液注入量200μL、溶媒流速1.0ml/分、溶媒温度40℃で測定を行い、ポリスチレン換算で質量平均分子量を算出することができる。この際に用いる標準ポリスチレンの質量平均分子量は、2000000、430000、110000、35000、10000、4000、600である。 The mass average molecular weight can be measured by the following method. The same applies to other resins.
Using gel permeation chromatography, measurement is made at a solvent chloroform, a solution concentration of 0.2 wt / vol%, a solution injection amount of 200 μL, a solvent flow rate of 1.0 ml / min, a solvent temperature of 40 ° C., and a mass average molecular weight in terms of polystyrene is obtained. Can be calculated. The mass average molecular weight of the standard polystyrene used in this case is 20000, 430000, 110000, 35000, 10000, 4000, 600.
ポリエステル系ホットメルト接着剤の原料モノマーとして用いられる二塩基酸の具体例としては、テレフタル酸、イソフタル酸、コハク酸、アジピン酸、セバシン酸、ドデカン二酸等が挙げられ、グリコールの具体例としてはエチレングリコール、プロピレングリコール、1,4-ブタンジオール、1,6-ヘキサンジオール、シクロヘキサンジオール、ポリオキシレングリコール等が挙げられる。
上記の中でも、アジピン酸や1,4-ブタンジオール等を分子骨格に含むポリエステル樹脂からなるホットメルト樹脂が好ましく用いられる。
市販されているポリエステル系ホットメルト樹脂として、例えば日本合成化学工業社製「ニチゴーポリエスター」シリーズや東洋紡績社製「バイロン」シリーズを挙げることができる。 Examples of the polyester hot melt resin used as the polyester resin (4-A) include a resin composition containing as a main component a polyester hot melt resin that is a polycondensation polymer of dibasic acid and glycol. .
Specific examples of dibasic acids used as raw material monomers for polyester hot melt adhesives include terephthalic acid, isophthalic acid, succinic acid, adipic acid, sebacic acid, dodecanedioic acid, etc. Specific examples of glycols Examples include ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, cyclohexanediol, and polyoxylene glycol.
Among the above, a hot melt resin made of a polyester resin containing adipic acid, 1,4-butanediol or the like in the molecular skeleton is preferably used.
Examples of commercially available polyester hot melt resins include “Nichigo Polyester” series manufactured by Nippon Synthetic Chemical Industry Co., Ltd. and “Byron” series manufactured by Toyobo Co., Ltd.
かかる観点から、ポリエステル系ホットメルト接着剤の質量平均分子量は、25,000以上であるのが特に好ましく、中でも30,000以上であるのがさらに好ましい。また、110,000以下であるのが特に好ましく、中でも100,000以下であるのがさらに好ましい。 The mass average molecular weight of the polyester hot melt adhesive is preferably 20,000 to 120,000. If it is this range, since it has a mechanical characteristic sufficient practically and melt viscosity is suitable, possibility that a problem will generate | occur | produce in a shaping | molding process is low.
From this viewpoint, the mass average molecular weight of the polyester-based hot melt adhesive is particularly preferably 25,000 or more, and more preferably 30,000 or more. Further, it is particularly preferably 110,000 or less, and more preferably 100,000 or less.
メラミンは、第1の難燃性樹脂組成物に用いるメラミンと同様であり、同様の作用を得ることができる。また、第1の難燃性樹脂組成物と同様に、第4の難燃性積層体の効果を損なわない範囲で、メラミンと他の難燃剤ないし難燃助剤を併用しても構わない。
メラミンは、燃焼時に不燃性のガスを発生するため、A層を難燃化することができるばかりか、B層をも難燃化することができ、第4の難燃性積層体全体の難燃性を格段に高めることができる。 (melamine)
Melamine is similar to the melamine used in the first flame retardant resin composition, and can obtain the same action. Similarly to the first flame retardant resin composition, melamine and other flame retardants or flame retardant aids may be used in combination as long as the effects of the fourth flame retardant laminate are not impaired.
Melamine generates a non-flammable gas during combustion, so that not only the A layer can be made flame retardant, but also the B layer can be made flame retardant, making it difficult for the entire fourth flame retardant laminate. The flammability can be greatly increased.
フェノキシ樹脂は、第2の難燃性樹脂組成物に用いるフェノキシ樹脂と同様であり、同様の作用を得ることができる。 (Phenoxy resin)
The phenoxy resin is the same as the phenoxy resin used in the second flame retardant resin composition, and the same action can be obtained.
A層を構成する樹脂組成物a中に占めるメラミンの配合割合は、20~80質量%であることが重要である。A層を構成する樹脂組成物a中に占めるメラミンの配合割合が20質量%以上であれば、十分な難燃性を得ることができる。一方、メラミンの配合割合が80質量%以下であれば第4の難燃性積層体の機械物性を損なうことがない。
かかる観点から、A層を構成する樹脂組成物a中に占めるメラミンの配合割合は、30質量%以上であるのが好ましく、中でも40質量%以上であるのがさらに好ましい。また、70質量%以下であるのが好ましく、中でも60質量%以下であるのがさらに好ましい。 (Mixing ratio)
It is important that the blending ratio of melamine in the resin composition a constituting the A layer is 20 to 80% by mass. If the blending ratio of melamine in the resin composition a constituting the A layer is 20% by mass or more, sufficient flame retardancy can be obtained. On the other hand, if the blending ratio of melamine is 80% by mass or less, the mechanical properties of the fourth flame retardant laminate will not be impaired.
From this viewpoint, the blending ratio of melamine in the resin composition a constituting the A layer is preferably 30% by mass or more, and more preferably 40% by mass or more. Moreover, it is preferable that it is 70 mass% or less, and it is still more preferable that it is 60 mass% or less especially.
かかる観点から、A層を構成する樹脂組成物a中に占めるフェノキシ樹脂の割合は5質量%以上であるのが好ましく、また、20質量%以下であるのが好ましい。 Regarding the blending amount of the phenoxy resin, it is important that the proportion of the phenoxy resin in the resin composition a constituting the A layer is 1 to 30% by mass. If it falls below this range, the effect of improving adhesion to metal is hardly obtained, and if it exceeds this range, mechanical properties, particularly impact resistance, may be reduced.
From this viewpoint, the ratio of the phenoxy resin in the resin composition a constituting the A layer is preferably 5% by mass or more, and preferably 20% by mass or less.
B層は、ポリエステル系樹脂(4-B)を主成分とする樹脂組成物bからなる層である。 <B layer>
The B layer is a layer made of the resin composition b mainly composed of a polyester resin (4-B).
ポリエステル系樹脂(4-B)としては、ガラス転移温度が50~120℃であり、且つ結晶融解熱量ΔHmが40~100J/gであるポリエステル系樹脂を用いることが重要である。この条件を満たすことにより、優れた耐熱性を有する積層体を提供することができる。 (Polyester resin (4-B))
As the polyester resin (4-B), it is important to use a polyester resin having a glass transition temperature of 50 to 120 ° C. and a crystal melting heat ΔHm of 40 to 100 J / g. By satisfying this condition, a laminate having excellent heat resistance can be provided.
かかる観点から、ポリエステル系樹脂(4-B)のガラス転移温度は、55℃以上であるのが好ましく、中でも60℃以上であるのがさらに好ましい。また、110℃以下であるのが好ましく、中でも100℃以下であるのがさらに好ましい。 It is important that the glass transition temperature of the polyester resin (4-B) is 50 to 120 ° C. as described above. When the glass transition temperature of the polyester resin (4-B) is 50 to 120 ° C., a laminate having excellent molding processability and excellent heat resistance during use can be obtained.
From such a viewpoint, the glass transition temperature of the polyester resin (4-B) is preferably 55 ° C. or higher, and more preferably 60 ° C. or higher. Moreover, it is preferable that it is 110 degrees C or less, and it is still more preferable that it is 100 degrees C or less especially.
かかる観点から、ポリエステル系樹脂(4-B)の結晶融解熱量ΔHmは、45J/g以上であるのが好ましく、中でも50J/g以上であるのがさらに好ましい。また、90J/g以下であるのが好ましく、中でも80J/g以下であるのがさらに好ましい。 It is important that the heat of crystal fusion ΔHm of the polyester resin (4-B) is 40 to 100 J / g as described above. When the heat of crystal melting ΔHm of the polyester resin (4-B) is 40 to 100 J / g, problems such as deformation during secondary processing do not occur.
From this viewpoint, the heat of crystal fusion ΔHm of the polyester resin (4-B) is preferably 45 J / g or more, and more preferably 50 J / g or more. Further, it is preferably 90 J / g or less, more preferably 80 J / g or less.
かかる観点から、ポリエステル系樹脂(4-B)の質量平均分子量は、35,000以上であるのが特に好ましく、中でも40,000以上であるのがさらに好ましい。また、75,000以下であるのが特に好ましく、中でも70,000以下であるのがさらに好ましい。 The mass average molecular weight of the polyester resin (4-B) is preferably 30,000 to 80,000. If the mass average molecular weight of the polyester-based resin (4-B) is 30,000 or more, an appropriate resin cohesive force can be obtained, and the strength and elongation of the laminate can be prevented from being insufficient or brittle. it can. On the other hand, if it is 80,000 or less, the melt viscosity can be lowered, which is preferable from the viewpoint of production and productivity improvement.
From this viewpoint, the mass average molecular weight of the polyester resin (4-B) is particularly preferably 35,000 or more, and more preferably 40,000 or more. Further, it is particularly preferably 75,000 or less, and more preferably 70,000 or less.
第4の難燃性積層体において、A層を構成する樹脂組成物a及びB層を構成する樹脂組成物bに、耐加水分解性を付与するためにカルボジイミド化合物を配合してもよい。但し、配合しなくてもよい。 <Other ingredients>
In the fourth flame-retardant laminate, a carbodiimide compound may be blended in the resin composition a constituting the A layer and the resin composition b constituting the B layer in order to impart hydrolysis resistance. However, it is not necessary to mix.
第4の難燃性積層体の全層厚に対するA層の層厚の割合は、20~70%であるのが好ましい。A層の層厚の割合を20%以上にすることにより、第4の難燃性積層体に十分な難燃性を付与することが可能である。一方、A層の層厚の割合を70%以下にすることにより第4の難燃性積層体に十分な機械特性を付与することができる。
かかる観点から、第4の難燃性積層体の全層厚に対するA層の層厚の割合は、25%以上であるのが特に好ましく、中でも30%以上であるのがさらに好ましい。また、60%以下であるのが特に好ましく、中でも50%以下であるのがさらに好ましい。 <Layer thickness>
The ratio of the layer thickness of the A layer to the total thickness of the fourth flame retardant laminate is preferably 20 to 70%. By setting the ratio of the layer thickness of the A layer to 20% or more, it is possible to impart sufficient flame retardancy to the fourth flame retardant laminate. On the other hand, by setting the ratio of the layer thickness of the A layer to 70% or less, sufficient mechanical properties can be imparted to the fourth flame retardant laminate.
From this viewpoint, the ratio of the layer thickness of the A layer to the total layer thickness of the fourth flame retardant laminate is particularly preferably 25% or more, and more preferably 30% or more. Further, it is particularly preferably 60% or less, and more preferably 50% or less.
第4の難燃性積層体において、A層とB層間の剥離強度は、23℃で3N/cm以上であるのが好ましく、特に4N/cm以上、中でも5N/cm以上であるのが好ましい。
また、第4の難燃性積層体のA層を金属に接着する場合、例えば配線ケーブルを作製する場合を想定すると、A層と金属(特に錫メッキ銅箔)との剥離強度は、23℃で5N/cm以上となり、特に好ましくは6N/cm以上、中でも好ましくは7N/cm以上となる。
中でも、A層とB層間の剥離強度が3N/cm以上で、かつ、A層と金属導体(特に錫メッキ銅箔)との剥離強度が5N/cm以上であれば、積層体として様々な用途に使用可能であるため、より一層好ましい。 <Peel strength>
In the fourth flame-retardant laminate, the peel strength between the A layer and the B layer is preferably 3 N / cm or more at 23 ° C., more preferably 4 N / cm or more, and particularly preferably 5 N / cm or more.
Further, when the A layer of the fourth flame retardant laminate is bonded to a metal, for example, assuming that a wiring cable is produced, the peel strength between the A layer and the metal (particularly tin-plated copper foil) is 23 ° C. 5 N / cm or more, particularly preferably 6 N / cm or more, and particularly preferably 7 N / cm or more.
In particular, if the peel strength between the A layer and the B layer is 3 N / cm or more and the peel strength between the A layer and the metal conductor (particularly tin-plated copper foil) is 5 N / cm or more, various uses as a laminate are possible. This is even more preferable.
第4の難燃性積層体は、前述した第3の難燃性積層体と同様に製造することができる。 <Manufacturing method>
The fourth flame retardant laminate can be produced in the same manner as the third flame retardant laminate described above.
第4の難燃性積層体は、難燃性、特にUL94垂直燃焼試験UL94VTMの判定基準のVTM-0規格を満たす難燃性を得ることができるばかりか、金属、特に銅との接着性に優れた金属接着性を得ることができるため、例えば、金属導体を被覆する被覆樹脂フィルムとして好適に使用することができる。すなわち、2枚の第4の難燃性積層体を用い、これらのA層間に金属導体を配置して2枚の第4の難燃性積層体を貼り合わせて配線ケーブルを作製することができる。
中でも特に、第4の難燃性積層体は、上記の如く、優れた難燃性と金属接着性を得ることができるばかりか、優れた柔軟性、優れた耐熱性をも得ることができるから、フラットケーブル用として特に適している。 <Application>
The fourth flame retardant laminate can not only achieve flame retardancy, particularly flame retardancy satisfying the V94-0 standard of UL94 vertical combustion test UL94VTM, but also adhere to metal, especially copper. Since excellent metal adhesiveness can be obtained, for example, it can be suitably used as a coating resin film for coating a metal conductor. That is, a wiring cable can be produced by using two fourth flame retardant laminates, placing metal conductors between these A layers, and bonding the four fourth flame retardant laminates together. .
In particular, the fourth flame retardant laminate can obtain not only excellent flame retardancy and metal adhesion as described above, but also excellent flexibility and excellent heat resistance. Especially suitable for flat cables.
次に、第5の実施形態に係る難燃性積層体(以下「第5の難燃性積層体」という)について説明する。 [Fifth flame retardant laminate]
Next, a flame retardant laminate according to a fifth embodiment (hereinafter referred to as “fifth flame retardant laminate”) will be described.
すなわち、第5の難燃性積層体は、ガラス転移温度が20℃以下のポリエステル系樹脂(5-A)、メラミンおよび架橋剤の混合物を主成分とするA層の少なくとも片側に、ガラス転移温度が60℃以上のポリエステル系樹脂(5-B)を主成分とするB層を有する積層体であり、前記積層体のゲル分率が15質量%以上、55質量%以下でありかつ積層体に占めるメラミンの割合が10質量%以上、40質量%以下であることを特徴とする耐熱性難燃積層体である。 The fifth flame-retardant laminate provides a laminate having excellent flame retardancy and excellent heat resistance and mechanical properties without containing a halogen-based compound and a phosphorus-based compound. .
That is, the fifth flame retardant laminate has a glass transition temperature on at least one side of the A layer mainly composed of a mixture of a polyester resin (5-A) having a glass transition temperature of 20 ° C. or lower, melamine and a crosslinking agent. Is a laminate having a B layer composed mainly of a polyester resin (5-B) at 60 ° C. or higher, the gel fraction of the laminate being 15% by mass or more and 55% by mass or less, and The heat-resistant flame-retardant laminate is characterized in that the proportion of melamine occupied is 10% by mass or more and 40% by mass or less.
ポリエステル系樹脂(5-A)は、ガラス転移温度が20℃以下であることが重要である。この条件を満たすことにより、ガラス転移温度が60℃で以上であるポリエステル系樹脂(5-B)からなるB層との接着性が良好であり、2次加工、および使用時における層間での剥離を生じることのない積層体を提供することができるだけでなく、優れた機械強度を有する積層体を提供することができる。また、ポリエステル系樹脂(5-A)は、単一の樹脂であっても、二種類以上の樹脂の混合物であってもよい。 (Polyester resin (5-A))
It is important that the polyester resin (5-A) has a glass transition temperature of 20 ° C. or lower. By satisfying this condition, the adhesiveness with the B layer made of the polyester resin (5-B) having a glass transition temperature of 60 ° C. or higher is good, and the secondary processing and peeling between the layers at the time of use are performed. It is possible not only to provide a laminate that does not cause the occurrence of the problem, but also to provide a laminate having excellent mechanical strength. The polyester resin (5-A) may be a single resin or a mixture of two or more resins.
なお、ポリエステル系樹脂(5-A)のガラス転移温度の下限値は特に限定されるものではないが、前記ガラス転移温度が-100℃以上であれば、全ての実用温度域において、ポリエステル系樹脂(5-B)からなるB層との優れた接着強度が得られる。
また、ポリエステル系樹脂(5-A)の結晶融解熱量ΔHmが40J/g以下、好ましくは35J/g以下、より好ましくは30J/g以下であれば、さらにB層との接着強度を向上することができる。 The glass transition temperature of the polyester resin (5-A) used for the fifth flame-retardant laminate is 20 ° C. or lower, preferably 10 ° C. or lower, and more preferably 0 ° C. or lower. If the glass transition temperature of the polyester-based resin (5-A) is 20 ° C. or lower, the problem of peeling from the B layer made of the polyester-based resin (5-B) during molding, secondary processing, and use Not only does not occur, but also excellent mechanical properties (particularly tensile elongation) can be imparted to the flame retardant laminate.
The lower limit of the glass transition temperature of the polyester resin (5-A) is not particularly limited, but the polyester resin can be used in all practical temperature ranges as long as the glass transition temperature is −100 ° C. or higher. Excellent adhesion strength with the B layer comprising (5-B) can be obtained.
Further, when the heat of crystal fusion ΔHm of the polyester resin (5-A) is 40 J / g or less, preferably 35 J / g or less, more preferably 30 J / g or less, the adhesive strength with the B layer can be further improved. Can do.
メラミンは、第1の難燃性樹脂組成物に用いるメラミンと同様であり、同様の作用を得ることができる。また、第1の難燃性樹脂組成物と同様に、第5の難燃性積層体の効果を損なわない範囲で、メラミンと他の難燃剤ないし難燃助剤を併用しても構わない。 (melamine)
Melamine is similar to the melamine used in the first flame retardant resin composition, and can obtain the same action. Similarly to the first flame retardant resin composition, melamine and other flame retardants or flame retardant aids may be used in combination as long as the effects of the fifth flame retardant laminate are not impaired.
第5の難燃性積層体に用いる架橋剤としては、分子内にアクリル基・メタクリル基・アリル基・ビニル基等の官能基を2個以上有する分子量が概ね2000以下の化合物が好適に使用できる。具体的には、ジアリルイソシアネート、トリアリルイソシアネート、ジメタアリルイソシアネート、トリメタアリルイソシアネート、ジアリルモノグリシジルイソシアネート、1,4-ブタンジオールジメタアクリレート、ポリエチレングリコールメタアクリレート、ペンタエリスリトールジメタアクリレート、ジペンタエリスリトールヘキサアクリレート、トリメチロールプロパンアクリレート、ジビニルベンゼン、トリビニルベンゼン、ヘキサメチルベンゼン等が挙げられる。 (Crosslinking agent)
As the cross-linking agent used in the fifth flame retardant laminate, a compound having a molecular weight of about 2000 or less and having two or more functional groups such as acryl group, methacryl group, allyl group and vinyl group in the molecule can be suitably used. . Specifically, diallyl isocyanate, triallyl isocyanate, dimethallyl isocyanate, trimethallyl isocyanate, diallyl monoglycidyl isocyanate, 1,4-butanediol dimethacrylate, polyethylene glycol methacrylate, pentaerythritol dimethacrylate, dipenta Examples include erythritol hexaacrylate, trimethylolpropane acrylate, divinylbenzene, trivinylbenzene, and hexamethylbenzene.
ポリエステル系樹脂(5-B)としては、ガラス転移温度が60℃以上であることが重要である。この条件を満たすことにより、優れた耐熱性を有する積層体を提供することができる。ポリエステル系樹脂(5-B)の具体例としては、多価カルボン酸と多価アルコールを重合して得られる芳香族ポリエステル、乳酸系樹脂等の脂肪族ポリエステルが挙げられる。 (Polyester resin (5-B))
As the polyester resin (5-B), it is important that the glass transition temperature is 60 ° C. or higher. By satisfying this condition, a laminate having excellent heat resistance can be provided. Specific examples of the polyester resin (5-B) include aliphatic polyesters such as aromatic polyesters and lactic acid resins obtained by polymerizing polyvalent carboxylic acids and polyhydric alcohols.
なお、ポリエステル系樹脂(5-B)のガラス転移温度の下限値は特に限定されるものではないが、前記ガラス転移温度が100℃以下であれば、十分な難燃性、耐熱性、機械特性を備えた積層体が得られる。
また、ポリエステル系樹脂(5-B)の結晶融解熱量ΔHmの下限値が、45J/g以上、好ましくは50J/g以上、さらに好ましくは、55J/g以上であれば、より耐熱性に優れた積層体を提供することができる。 The lower limit value of the glass transition temperature of the polyester resin (5-B) is 60 ° C. or higher, preferably 65 ° C. or higher, and more preferably 70 ° C. or higher. If the lower limit of the glass transition temperature of the polyester resin (5-B) is 60 ° C. or higher, there will be no problem of insufficient heat resistance during secondary processing and use.
The lower limit of the glass transition temperature of the polyester-based resin (5-B) is not particularly limited. However, if the glass transition temperature is 100 ° C. or less, sufficient flame retardancy, heat resistance, mechanical properties are obtained. Is obtained.
Further, when the lower limit value of the heat of crystal fusion ΔHm of the polyester resin (5-B) is 45 J / g or more, preferably 50 J / g or more, more preferably 55 J / g or more, the heat resistance is further improved. A laminate can be provided.
第5の難燃性積層体の全層厚に対するA層の厚さの割合は、全積層体を構成する樹脂組成物中に占めるメラミンの割合が10質量%以上、40質量%以下となるように適宜調整することが可能であるが、層厚は、通常20%以上、好ましくは25%以上、さらに好ましくは30%以上であり、70%以下、好ましくは60%以下、さらに好ましくは50%以下である。A層の層厚の割合を20%以上、70%以下とすることにより、難燃性積層体に十分な難燃性、耐熱性、機械特性を付与することができる。 <Layer structure>
The ratio of the thickness of layer A to the total thickness of the fifth flame-retardant laminate is such that the proportion of melamine in the resin composition constituting the entire laminate is 10% by mass or more and 40% by mass or less. The layer thickness is usually 20% or more, preferably 25% or more, more preferably 30% or more, 70% or less, preferably 60% or less, more preferably 50%. It is as follows. By setting the ratio of the layer thickness of the A layer to 20% or more and 70% or less, sufficient flame retardancy, heat resistance, and mechanical properties can be imparted to the flame retardant laminate.
第5の難燃性積層体にさらに耐加水分解性を付与するために、カルボジイミド化合物を配合することができる。但し、配合しなくてもよい。
配合するカルボジイミド化合物の種類は、第1の難燃性樹脂組成物において説明した配合するカルボジイミド化合物と同様である。 <Carbodiimide compound>
In order to further impart hydrolysis resistance to the fifth flame retardant laminate, a carbodiimide compound can be blended. However, it is not necessary to mix.
The kind of carbodiimide compound to mix | blend is the same as the carbodiimide compound to mix | blend demonstrated in the 1st flame retardant resin composition.
添加量が多すぎる場合には、成型加工性が低下する場合がある Among these, slipperiness is achieved when inorganic particles such as silica, colloidal silica, alumina, alumina sol, kaolin, talc, mica, calcium carbonate, barium sulfate, carbon black, zeolite, titanium oxide, and metal fine powder are added. It is preferable because scratch resistance and the like are improved. The average particle size of the inorganic particles is preferably 0.005 μm or more and 5 μm or less, and more preferably 0.05 μm or more and 1 μm or less. Moreover, the addition amount is 0.05 mass% or more with respect to each of the resin composition which comprises A layer, B layer, or the resin composition which comprises the adhesive layer of A layer and B layer, 20 It is preferable to mix | blend in the ratio of the weight% or less, and it is more preferable to mix | blend in the ratio of 0.1 to 10 weight%.
If the amount added is too large, moldability may decrease.
第5の難燃性積層体は、前述した第3の難燃性積層体と同様に製造することができる。
但し、第5の難燃性積層体は、A層およびB層、A層また、はB層を延伸することが可能である。A層および/また、はB層の延伸倍率は、MD(長手方向)に1.5倍、このましくは3倍、さらにこのましくは5倍、TD(横手方向)に1.5倍、このましくは3倍、さらにこのましくは5倍である。また、延伸はMDおよび/また、はTDに行うことができるが、耐熱性、機械特性の向上の観点からMDおよびTDに延伸することが好ましい。 <Manufacturing method>
The fifth flame retardant laminate can be produced in the same manner as the third flame retardant laminate described above.
However, in the fifth flame-retardant laminate, the A layer and the B layer, the A layer, or the B layer can be stretched. The stretch ratio of the A layer and / or the B layer is 1.5 times in MD (longitudinal direction), preferably 3 times, more preferably 5 times, and 1.5 times in TD (lateral direction). This is 3 times, more preferably 5 times. The stretching can be performed in MD and / or TD, but it is preferable to stretch in MD and TD from the viewpoint of improving heat resistance and mechanical properties.
第5の難燃性積層体は、優れた難燃性、耐熱性、機械特性を兼ね備えているため、電気絶縁材、メンブレンスイッチ回路印刷基材、複写機内部部材、面状発熱体基材、FPC補強板等の用途に用いることができる。 <Application>
The fifth flame retardant laminate has excellent flame retardancy, heat resistance, and mechanical properties. Therefore, an electrical insulating material, a membrane switch circuit printing substrate, a copier internal member, a planar heating element substrate, It can be used for applications such as FPC reinforcing plates.
(1)積層体から切り取った0.25gの試験片をクロロホルム20mlに、23℃で5時間溶解させる。
(2)前記(1)で作製した溶液をSigma Laborzentrifugen GmbH社製テーブルトップ高速冷却遠心機3-18Kを用いて、回転速度11,400rpmで不溶解物の分離を行う。
(3)前記(2)で得られた不溶解物を乾燥し、樹脂成分以外の成分(例えばメラミン、無機物)を差し引いた後、以下の式にてゲル分率を算出する。 In addition, the gel fraction of the resin composition which comprises a 5th flame retardant laminated body is a value measured as follows.
(1) A test piece of 0.25 g cut from the laminate is dissolved in 20 ml of chloroform at 23 ° C. for 5 hours.
(2) The solution prepared in the above (1) is separated into insoluble matters at a rotation speed of 11,400 rpm using a table top high-speed cooling centrifuge 3-18K manufactured by Sigma Laborentrifugen GmbH.
(3) After drying the insoluble matter obtained in (2) above and subtracting components other than the resin component (for example, melamine, inorganic matter), the gel fraction is calculated by the following equation.
A:前記(3)にて得られた樹脂成分以外の成分(例えばメラミン、無機物)の質量を差し引いた後の樹脂成分の不溶解物の質量。
B:積層体中に占める樹脂成分以外の成分(例えばメラミン、無機物)の質量を差し引いた樹脂成分の理論質量。
なお、メラミンの配合量が予め分からない時は、IR(赤外吸収分析)測定によりメラミンのトリアジン環由来のピーク(815cm-1)の強度によりメラミンの添加量の算定を行えばよい。また、無機物質の配合量が予め分からない場合は、元素分析で無機元素の総和から無機物資の添加量の算定を行えばよい。 Gel fraction (mass%) = A / B × 100
A: The mass of the insoluble matter of the resin component after subtracting the mass of the components other than the resin component obtained in (3) (for example, melamine, inorganic).
B: Theoretical mass of the resin component obtained by subtracting the mass of components other than the resin component in the laminate (for example, melamine, inorganic).
When the blending amount of melamine is not known in advance, the amount of melamine added may be calculated from the intensity of the peak (815 cm-1) derived from the triazine ring of melamine by IR (infrared absorption analysis) measurement. In addition, when the blending amount of the inorganic substance is not known in advance, the addition amount of the inorganic material may be calculated from the sum of the inorganic elements by elemental analysis.
次に、第6の実施形態に係る難燃性積層体(以下「第6の難燃性積層体」という)について説明する。 [Sixth flame retardant laminate]
Next, a flame retardant laminate according to a sixth embodiment (hereinafter referred to as “sixth flame retardant laminate”) will be described.
メラミンは、燃焼時に不燃性のガスを発生するため、接着層を難燃化することができるばかりか、難燃剤を配合してない外層(B層)をも難燃化することができるため、積層体全体の難燃性を格別に高めることができる。さらに、メラミンと炭化促進剤を配合することで、燃焼時に速やかに樹脂の炭化が進行し、UL1581VW-1規格を満足することができる配線ケーブル用積層体を提供することができる。 This sixth flame-retardant laminate can express a higher degree of flame retardancy by blending melamine and a carbonization accelerator in a specific polyester resin constituting the adhesive layer (A layer). . In addition, since it does not contain a halogen compound and a phosphorus compound, it is possible to provide a material with excellent safety that does not cause problems such as environmental pollution.
Since melamine generates nonflammable gas when burned, not only can the adhesive layer be flame retardant, but also the outer layer (B layer) that does not contain a flame retardant can also be flame retardant. The flame retardance of the entire laminate can be significantly increased. Furthermore, by blending melamine and a carbonization accelerator, carbonization of the resin proceeds rapidly during combustion, and a wiring cable laminate capable of satisfying the UL1581VW-1 standard can be provided.
ここで、「A層上に」とは、A層上に直にB層を積層する場合のほか、A層上に他の層を介してB層を積層する場合を包含する。
以下、詳細に説明する。 Now, the sixth flame retardant laminate comprises a polyester resin (6-A) on a layer A composed of a resin composition a having a polyester resin (6-A), a mixture of melamine and a carbonization accelerator as main components. It is a laminated body provided with B layer which consists of the resin composition b which has B) as a main component.
Here, “on the A layer” includes not only the case where the B layer is laminated directly on the A layer, but also the case where the B layer is laminated on the A layer via another layer.
Details will be described below.
第6の難燃性積層体においてA層は、接着層の役割を備えた層であり、このA層は、ポリエステル系樹脂(6-A)、メラミンおよび炭化促進剤からなる混合物を主成分とする樹脂組成物aからなる層である。 <A layer>
In the sixth flame-retardant laminate, the A layer is a layer having a role of an adhesive layer, and this A layer is mainly composed of a mixture comprising a polyester resin (6-A), melamine and a carbonization accelerator. It is the layer which consists of the resin composition a to do.
ポリエステル系樹脂(6-A)は、ガラス転移温度が30℃以下である樹脂であることが重要である。ポリエステル系樹脂(6-A)のガラス転移温度が30℃以下であれば、低温から通常の使用温度までの広範囲において、優れた機械特性を有する積層体とすることができる。
かかる観点から、ポリエステル系樹脂(6-A)のガラス転移温度は、好ましくは-80℃以上、さらに好ましくは-70℃以上、特に好ましく-60℃以上である。また、20℃以下であるのが好ましく、特に10℃以下であることが好ましい。 (Polyester resin (6-A))
It is important that the polyester resin (6-A) is a resin having a glass transition temperature of 30 ° C. or lower. If the glass transition temperature of the polyester resin (6-A) is 30 ° C. or lower, a laminate having excellent mechanical properties can be obtained in a wide range from a low temperature to a normal use temperature.
From such a viewpoint, the glass transition temperature of the polyester resin (6-A) is preferably −80 ° C. or higher, more preferably −70 ° C. or higher, and particularly preferably −60 ° C. or higher. Moreover, it is preferable that it is 20 degrees C or less, and it is especially preferable that it is 10 degrees C or less.
かかる観点から、ポリエステル系樹脂(6-A)の結晶融解熱量ΔHmは8J/g以上であるのが好ましく、10J/g以上であるのがさらに好ましい。また、25J/g以下であるのが好ましく、20J/g以下であるのがさらに好ましい。 The polyester resin (6-A) is preferably a resin having a heat of crystal fusion ΔHm of 5 to 30 J / g. When the heat of crystal melting ΔHm of the polyester resin (6-A) is 5 to 30 J / g, a laminate having sufficient adhesiveness and heat resistance at the time of molding, secondary processing and use, can do.
From this viewpoint, the heat of crystal fusion ΔHm of the polyester-based resin (6-A) is preferably 8 J / g or more, and more preferably 10 J / g or more. Moreover, it is preferable that it is 25 J / g or less, and it is further more preferable that it is 20 J / g or less.
かかる観点から、脂肪族ポリエステルおよび芳香族脂肪族ポリエステルの質量平均分子量は、80,000以上であるのが好ましく、100,000以上であるのがさらに好ましい。また、300,000以下であるのが好ましく、250,000以下であるのがさらに好ましい。 These aliphatic polyesters and aromatic aliphatic polyesters preferably have a mass average molecular weight of 50,000 to 400,000. If the mass average molecular weight of these polyesters is 50,000 or more, there is no problem that the laminate is damaged due to insufficient flame retardancy or insufficient mechanical strength. Moreover, if a mass average molecular weight is 400,000 or less, the problem of the shaping | molding defect by the viscosity of resin being too high will not generate | occur | produce.
From this viewpoint, the mass average molecular weight of the aliphatic polyester and the aromatic aliphatic polyester is preferably 80,000 or more, and more preferably 100,000 or more. Moreover, it is preferable that it is 300,000 or less, and it is further more preferable that it is 250,000 or less.
メラミンは、第1の難燃性樹脂組成物に用いるメラミンと同様であり、同様の作用を得ることができる。また、第1の難燃性樹脂組成物と同様に、第5の難燃性積層体の効果を損なわない範囲で、メラミンと他の難燃剤ないし難燃助剤を併用しても構わない。 (melamine)
Melamine is similar to the melamine used in the first flame retardant resin composition, and can obtain the same action. Similarly to the first flame retardant resin composition, melamine and other flame retardants or flame retardant aids may be used in combination as long as the effects of the fifth flame retardant laminate are not impaired.
炭化促進剤としては、燃焼時において樹脂の炭化を促進することができる無機物あるいは、有機物であり、具体例としては、ペンタエリトリトール、ジペンタエリトリトール、トリペンタエリトリトール等の多価アルコール、スルファミン酸グアニジン、リン酸グアニジン等のグアニジン化合物、硫酸メラミン、硫酸アンモニウム等の硫酸化合物、硝酸メラミン、硝酸アンモニウム等の硝酸化合物、水酸基を有するフェノキシ樹脂、シリコーンオイル、シリコーンゴム、シリコーンレジン等のシリコーン化合物、メラミンシアヌレート、水酸化カルシウム、水酸化アルミニウム、水酸化マグネシウム、カルシウム・アルミネート水和物、酸化スズ水和物等の金属水酸化物、およびタルク、マイカ、ホウ酸亜鉛、酸化亜鉛、酸化マグネシウム等が挙げられる。この中でも特に、フェノキシ樹脂を使用することで、優れた炭化促進効果に加えて、金属との接着強度も向上することができる。なお、上記炭化促進剤は単独、あるいは、2種類以上を混合して用いることができる。 (Carbonization accelerator)
The carbonization accelerator is an inorganic substance or an organic substance that can promote carbonization of the resin at the time of combustion. Specific examples include polyhydric alcohols such as pentaerythritol, dipentaerythritol, tripentaerythritol, guanidine sulfamate, Guanidine compounds such as guanidine phosphate, sulfuric acid compounds such as melamine sulfate and ammonium sulfate, nitric acid compounds such as melamine nitrate and ammonium nitrate, phenoxy resins having a hydroxyl group, silicone oil, silicone rubber, silicone compounds such as silicone resin, melamine cyanurate, water Metal hydroxides such as calcium oxide, aluminum hydroxide, magnesium hydroxide, calcium / aluminate hydrate, tin oxide hydrate, talc, mica, zinc borate, zinc oxide, magnesium oxide, etc. And the like. Among these, in particular, by using a phenoxy resin, in addition to an excellent carbonization promoting effect, the adhesive strength with a metal can also be improved. In addition, the said carbonization promoter can be used individually or in mixture of 2 or more types.
フェノキシ樹脂は、第2の難燃性樹脂組成物に用いるフェノキシ樹脂と同様であり、同様の作用を得ることができる。 (Phenoxy resin)
The phenoxy resin is the same as the phenoxy resin used in the second flame retardant resin composition, and the same action can be obtained.
第6の難燃性積層体においては、A層を構成する樹脂組成物a中に占めるメラミンの配合割合は、20~80質量%であることが重要である。A層を構成する樹脂組成物a中に占めるメラミンの配合割合が20質量%以上であれば、十分な難燃性を得ることができる。一方、メラミンの配合割合が80質量%以下であれば第6の難燃性積層体の機械物性を損なうことがない。
かかる観点から、A層を構成する樹脂組成物a中に占めるメラミンの配合割合は、30質量%以上であるのが好ましく、中でも40質量%以上であるのがさらに好ましい。また、70質量%以下であるのが好ましく、中でも60質量%以下であるのがさらに好ましい。 <Combination ratio>
In the sixth flame-retardant laminate, it is important that the blending ratio of melamine in the resin composition a constituting the A layer is 20 to 80% by mass. If the blending ratio of melamine in the resin composition a constituting the A layer is 20% by mass or more, sufficient flame retardancy can be obtained. On the other hand, if the blending ratio of melamine is 80% by mass or less, the mechanical properties of the sixth flame retardant laminate will not be impaired.
From this viewpoint, the blending ratio of melamine in the resin composition a constituting the A layer is preferably 30% by mass or more, and more preferably 40% by mass or more. Moreover, it is preferable that it is 70 mass% or less, and it is still more preferable that it is 60 mass% or less especially.
かかる観点から、A層を構成する樹脂組成物a中に占めるメラミンの配合割合は、1質量%以上であるのが好ましく、中でも5質量%以上であるのがさらに好ましい。また、30質量%以下であるのが好ましく、中でも20質量%以下であるのがさらに好ましい。 It is important that the blending ratio of the carbonization accelerator in the resin composition a constituting the A layer is 1 to 30% by mass. When the blending ratio of the carbonization accelerator in the resin composition a constituting the A layer is 1% by mass or more, a sufficient carbonization promoting effect can be obtained. On the other hand, if the blending ratio of melamine is 30% by mass or less, the mechanical properties of the sixth flame retardant laminate will not be impaired.
From this viewpoint, the blending ratio of melamine in the resin composition a constituting the A layer is preferably 1% by mass or more, and more preferably 5% by mass or more. Moreover, it is preferable that it is 30 mass% or less, and it is still more preferable that it is 20 mass% or less especially.
B層は、ポリエステル系樹脂(6-B)を主成分とする樹脂組成物bからなる層である。 <B layer>
The B layer is a layer made of the resin composition b mainly composed of a polyester resin (6-B).
ポリエステル系樹脂(6-B)としては、ガラス転移温度が50~120℃であり、且つ結晶融解熱量ΔHmが40~100J/gであるポリエステル系樹脂を用いることが重要である。この条件を満たすことにより、優れた耐熱性を有する積層体を提供することができる。 (Polyester resin (6-B))
As the polyester resin (6-B), it is important to use a polyester resin having a glass transition temperature of 50 to 120 ° C. and a crystal melting heat ΔHm of 40 to 100 J / g. By satisfying this condition, a laminate having excellent heat resistance can be provided.
かかる観点から、ポリエステル系樹脂(6-B)のガラス転移温度は、55℃以上であるのが好ましく、中でも60℃以上であるのがさらに好ましい。また、110℃以下であるのが好ましく、中でも100℃以下であるのがさらに好ましい。 It is important that the glass transition temperature of the polyester resin (6-B) is 50 to 120 ° C. as described above. When the glass transition temperature of the polyester resin (6-B) is 50 to 120 ° C., a laminate having excellent moldability and excellent heat resistance during use can be obtained.
From this viewpoint, the glass transition temperature of the polyester resin (6-B) is preferably 55 ° C. or higher, and more preferably 60 ° C. or higher. Moreover, it is preferable that it is 110 degrees C or less, and it is still more preferable that it is 100 degrees C or less especially.
かかる観点から、ポリエステル系樹脂(6-B)の結晶融解熱量ΔHmは、45J/g以上であるのが好ましく、中でも50J/g以上であるのがさらに好ましい。また、90J/g以下であるのが好ましく、中でも80J/g以下であるのがさらに好ましい。 It is important that the heat of crystal fusion ΔHm of the polyester resin (6-B) is 40 to 100 J / g as described above. When the heat of crystal fusion ΔHm of the polyester resin (6-B) is 40 to 100 J / g, problems such as deformation during secondary processing do not occur.
From this point of view, the heat of crystal fusion ΔHm of the polyester resin (6-B) is preferably 45 J / g or more, and more preferably 50 J / g or more. Further, it is preferably 90 J / g or less, more preferably 80 J / g or less.
かかる観点から、ポリエステル系樹脂(6-B)の質量平均分子量は、35,000以上であるのが特に好ましく、中でも40,000以上であるのがさらに好ましい。また、75,000以下であるのが特に好ましく、中でも70,000以下であるのがさらに好ましい。 The mass average molecular weight of the polyester resin (6-B) is preferably 30,000 to 80,000. If the mass average molecular weight of the polyester-based resin (6-B) is 30,000 or more, an appropriate resin cohesive force can be obtained, and it is possible to prevent the laminate from being insufficient in strength or brittle. it can. On the other hand, if it is 80,000 or less, the melt viscosity can be lowered, which is preferable from the viewpoint of production and productivity improvement.
From this viewpoint, the mass average molecular weight of the polyester resin (6-B) is particularly preferably 35,000 or more, and more preferably 40,000 or more. Further, it is particularly preferably 75,000 or less, and more preferably 70,000 or less.
第6の難燃性積層体において、A層を構成する樹脂組成物aおよびB層を構成する樹脂組成物bに、耐加水分解性を付与するためにカルボジイミド化合物を配合してもよい。但し、配合しなくてもよい。 <Other ingredients>
In the sixth flame-retardant laminate, a carbodiimide compound may be blended with the resin composition a constituting the A layer and the resin composition b constituting the B layer in order to impart hydrolysis resistance. However, it is not necessary to mix.
第6の難燃性積層体の全層厚に対するA層の層厚の割合は、20~70%であるのが好ましい。A層の層厚の割合を20%以上にすることにより、第6の難燃性積層体に十分な難燃性を付与することが可能である。一方、A層の層厚の割合を70%以下にすることにより第6の難燃性積層体に十分な機械特性を付与することができる。
かかる観点から、第6の難燃性積層体の全層厚に対するA層の層厚の割合は、25%以上であるのが特に好ましく、中でも30%以上であるのがさらに好ましい。また、60%以下であるのが特に好ましく、中でも50%以下であるのがさらに好ましい。 <Layer thickness>
The ratio of the layer thickness of the A layer to the total thickness of the sixth flame retardant laminate is preferably 20 to 70%. By setting the ratio of the layer thickness of the A layer to 20% or more, it is possible to impart sufficient flame retardancy to the sixth flame retardant laminate. On the other hand, by setting the ratio of the layer thickness of the A layer to 70% or less, sufficient mechanical properties can be imparted to the sixth flame-retardant laminate.
From this viewpoint, the ratio of the layer thickness of the A layer to the total layer thickness of the sixth flame retardant laminate is particularly preferably 25% or more, and more preferably 30% or more. Further, it is particularly preferably 60% or less, and more preferably 50% or less.
第6の難燃性積層体は、非常に優れた難燃性を有し、難燃性を評価する一つの指標であるUL1581VW-1を満たすことが可能である。すなわち、第6の難燃性積層体は、一定の条件を満たすポリエステル系樹脂(A)とメラミン、炭化促進剤を主成分としてA層を構成し、一定の条件を満たすポリエステル系樹脂(6-B)を主成分としてB層を構成することにより、UL1581VW-1を満たすことが可能となる。 <Flame retardance>
The sixth flame-retardant laminate has very excellent flame retardancy, and can satisfy UL1581VW-1, which is one index for evaluating the flame retardancy. That is, the sixth flame retardant laminate comprises a polyester resin (A) satisfying a certain condition, a layer A composed mainly of melamine and a carbonization accelerator, and a polyester resin (6- By configuring the B layer with B) as a main component, it is possible to satisfy UL1581VW-1.
第6の難燃性積層体は、前述した第3の難燃性積層体と同様に製造することができる。 <Manufacturing method>
The sixth flame retardant laminate can be produced in the same manner as the third flame retardant laminate described above.
第6の難燃性積層体は、難燃性、特にUL1581VW-1規格を満たす難燃性を得ることができ、例えば、配線ケーブルを被覆する被覆樹脂フィルムとして好適に使用することができる。すなわち、2枚の第6の難燃性積層体を用い、これらのA層間に金属導体を配置して2枚の本積層体を貼り合わせて配線ケーブルを作製することができる。
中でも特に、第6の難燃性積層体は、上記の如く、優れた難燃性を得ることができるばかりか、優れた柔軟性、優れた耐熱性をも得ることができるから、フラットケーブル用として特に適している。 <Application>
The sixth flame-retardant laminate can obtain flame retardancy, particularly flame retardancy satisfying the UL1581VW-1 standard, and can be suitably used, for example, as a covering resin film for covering a wiring cable. That is, a wiring cable can be produced by using two sixth flame retardant laminates, placing metal conductors between these A layers, and bonding the two laminates together.
In particular, the sixth flame-retardant laminate can obtain not only excellent flame retardancy but also excellent flexibility and excellent heat resistance as described above. Particularly suitable as.
本発明において「主成分」と表現した場合には、特に記載しない限り、当該主成分の機能を妨げない範囲で他の成分を含有することを許容する意を包含するものである。特に当該主成分の含有割合を特定するものではないが、その成分(2成分以上が主成分である場合には、これらの合計量)が組成物中で60質量%以上、特に70質量%以上、中でも90質量%以上(100%含む)を占めるのが好ましい。例えば、樹脂組成物a中の混合物は、樹脂組成物a中で60質量%以上、特に70質量%以上、中でも90質量%以上(100%含む)を占めるのが好ましい。 [Explanation of terms]
In the present invention, the expression “main component” includes the meaning of allowing other components to be contained within a range that does not hinder the function of the main component unless otherwise specified. Although the content ratio of the main component is not particularly specified, its component (when two or more components are main components, the total amount thereof) is 60% by mass or more, particularly 70% by mass or more in the composition. Of these, 90% by mass or more (including 100%) is preferable. For example, the mixture in the resin composition a preferably occupies 60% by mass or more, particularly 70% by mass or more, particularly 90% by mass or more (including 100%) in the resin composition a.
また、「X以上」(Xは任意の数字)或いは「Y以下」(Yは任意の数字)と記載した場合、「Xより大きいことが好ましい」或いは「Y未満であるのが好ましい」旨の意図も包含する。 Further, in this specification, when “X to Y” (X and Y are arbitrary numbers) is described, it means “X or more and Y or less” unless otherwise specified. The meaning of “preferably smaller than Y” is included.
In addition, when “X or more” (X is an arbitrary number) or “Y or less” (Y is an arbitrary number), it is “preferably greater than X” or “preferably less than Y”. Includes intentions.
(1)ポリエステル系樹脂を5mm直径の10mg程度の鱗片状にして、試験サンプルとする。
(2)前記(1)で得られた試験サンプルを、示差走査熱量計(パーキンエルマー製DSC-7)によりJIS-K7121に基づいて試験片を200℃で2分保持した後、10℃/分の速度にて-40℃まで降温する。次いで、-40℃から200℃まで10℃/分にて昇温測定を行う。なお、一連の測定は窒素雰囲気下にて行なう。
(3)前記(2)の測定により得られたサーモグラムよりガラス転移温度および結晶融解熱量を読み取る。 The “glass transition temperature” and “crystal heat of fusion” of the polyester resin in the present invention are values measured as follows. In Examples and Comparative Examples described later, the measurement was performed by the method described below unless otherwise specified.
(1) A polyester-based resin is formed into a scale of about 10 mg having a diameter of 5 mm and used as a test sample.
(2) The test sample obtained in (1) above was held at 200 ° C. for 2 minutes based on JIS-K7121 using a differential scanning calorimeter (DSC-7 manufactured by Perkin Elmer), and then 10 ° C./min The temperature is decreased to −40 ° C. Next, the temperature rise is measured from −40 ° C. to 200 ° C. at 10 ° C./min. A series of measurements are performed in a nitrogen atmosphere.
(3) The glass transition temperature and the heat of crystal melting are read from the thermogram obtained by the measurement of (2).
但し、本発明の範囲が以下の実施例に限定されるものではない。 Examples and comparative examples corresponding to the first and second embodiments (flame retardant polyester resin compositions) and the third to sixth embodiments (flame retardant laminates) described above, respectively. Will be described.
However, the scope of the present invention is not limited to the following examples.
先ず、第1の実施形態に係る実施例及び比較例について説明する。 [Example and Comparative Example of First Embodiment]
First, examples and comparative examples according to the first embodiment will be described.
厚みが200μm以下の場合は、長さ200mm×幅50mmの評価用サンプル、厚みが200μmを超える場合は、長さ127mm×幅13mm(厚みはそれぞれの試験片により異なる)の評価用サンプルを用いて、Underwriters Laboratories社の安全標準UL94薄手材料垂直燃焼試験(サンプル厚みが200μm以下の場合)、及び、UL94垂直燃焼試験(サンプル厚みが200μmを超える場合)の手順に基づき、試験回数5回にて燃焼試験を実施し、燃焼の様子(特に燃焼中における滴下物の有無)を観察すると共に燃焼時間(試験回数5回の合計燃焼時間)を測定した。
UL94垂直燃焼試験において、厚みが200μm以下のサンプルについては、UL94VTMの判定基準に基づき、VTM-0、1、2の規格を満たすか否か判例し、VTM-2を満たさないものは規格外と評価し、VTM-0を満たすものを合格品と評価した。また、厚みが200μmを超えるサンプルについては、UL94Vの判定基準に基づき、VTM-0、1、2の規格を満たすか否か判例し、VTM-2を満たさないものは規格外と評価し、VTM-0を満たすものを合格品と評価した。 (1) Flame retardance When the thickness is 200 μm or less, an evaluation sample having a length of 200 mm × width 50 mm, and when the thickness exceeds 200 μm, the length is 127 mm × width 13 mm (thickness varies depending on each test piece). Test using the sample for evaluation based on the procedures of Underwriters Laboratories Safety Standard UL94 Thin Material Vertical Combustion Test (when the sample thickness is 200 μm or less) and UL94 Vertical Combustion Test (when the sample thickness exceeds 200 μm) A combustion test was carried out at 5 times, and the state of combustion (particularly, the presence or absence of dripping material during combustion) was observed and the combustion time (total combustion time of 5 tests) was measured.
In the UL94 vertical combustion test, samples with a thickness of 200 μm or less are judged on the basis of the UL94VTM criteria whether or not the VTM-0, 1 and 2 standards are satisfied. A product satisfying VTM-0 was evaluated as an acceptable product. For samples with a thickness exceeding 200 μm, whether or not the standards of VTM-0, 1 and 2 are satisfied is judged based on the UL94V criteria, and those not satisfying VTM-2 are evaluated as nonstandard. Those satisfying −0 were evaluated as acceptable products.
長さ200mm×幅20mmの評価用サンプルを用いて、JIS C 2318に基づき、引張破断強度、引張破断伸度の測定を行った。破断時の強度と伸びを測定しn=5での平均値を求めた。雰囲気温度23℃、相対湿度50%、引張り速度200mm/min、つかみ間隔100mmにて測定を行い、破断時の強度と伸度を測定し、n=5での平均値を求めた。
引張強度は10MPa以上、引張伸度は10%以上を合格と評価した。 (2) Tensile strength and tensile elongation Using an evaluation sample having a length of 200 mm and a width of 20 mm, the tensile break strength and the tensile break elongation were measured based on JIS C 2318. The strength and elongation at break were measured, and the average value at n = 5 was determined. Measurement was performed at an ambient temperature of 23 ° C., a relative humidity of 50%, a pulling speed of 200 mm / min, and a gripping interval of 100 mm, and the strength and elongation at break were measured, and the average value at n = 5 was obtained.
A tensile strength of 10 MPa or more and a tensile elongation of 10% or more were evaluated as acceptable.
JIS K7121に基づき、10mg程度に削り出したサンプルについて、パーキンエルマー社製DSC-7を用いてポリエステル系樹脂の結晶融解熱量ΔHmの測定を行った。測定手順を以下に示す。 (3) Heat of crystal melting (ΔHm)
Based on JIS K7121, the crystal melting heat ΔHm of the polyester resin was measured using DSC-7 manufactured by Perkin Elmer Co., Ltd. The measurement procedure is shown below.
b.次に、10℃/分の速度にて200℃から30℃まで降温測定を行った。
c.さらに、10℃/分の速度にて30℃から200℃まで昇温測定を行った。 a. The temperature was raised from 30 ° C. to 200 ° C. at a rate of 500 ° C./min, and then held at 200 ° C. for 2 minutes.
b. Next, the temperature drop was measured from 200 ° C. to 30 ° C. at a rate of 10 ° C./min.
c. Furthermore, the temperature rise measurement was performed from 30 ° C. to 200 ° C. at a rate of 10 ° C./min.
長さ200mm×幅20mmの評価用サンプルの片側端部を固定して、ベーキング試験装置(大栄科学精器製作所製DKS-5S)内で垂直に保持し、140℃で1時間加熱した。加熱後のサンプルの外観を目視にて観察し、加熱前と比較して著しい変化がないものを○、加熱前と比較して収縮、シワ、著しい変形等が生じているものを×とした。 (4) Heat resistance One end of an evaluation sample having a length of 200 mm and a width of 20 mm is fixed and held vertically in a baking test apparatus (DKS-5S manufactured by Daiei Kagaku Seisaku Seisakusho) at 140 ° C for 1 hour. Heated. The appearance of the sample after heating was visually observed. A sample having no significant change compared to that before heating was marked with ◯, and a sample showing shrinkage, wrinkles, significant deformation, etc. compared with before heating was marked with ×.
次に、実施例・比較例で用いた原料、すなわちポリエステル系樹脂(A)、ポリエステル系樹脂(B)、メラミンについて説明する。 <Raw material>
Next, the raw materials used in Examples and Comparative Examples, that is, polyester resin (A), polyester resin (B), and melamine will be described.
製品名:東洋紡績社製バイロンバイロンGM-443
組成:多価カルボン酸成分=テレフタル酸53mol%、イソフタル酸38mol%、アジピン酸9mol%、多価アルコール成分=1,4-ブタンジオール100mol%
物性値:質量平均分子量=47,000、Tg=26℃、Tm=145℃、ΔHm=22.8J/g [Polyester resin (A) -1]
Product name: Byron Byron GM-443 manufactured by Toyobo Co., Ltd.
Composition: polycarboxylic acid component = 53 mol% terephthalic acid, 38 mol% isophthalic acid, 9 mol% adipic acid, polyhydric alcohol component = 100 mol% 1,4-butanediol
Physical property values: mass average molecular weight = 47,000, Tg = 26 ° C., Tm = 145 ° C., ΔHm = 22.8 J / g
製品名:東洋紡績社製バイロンGA-1300
組成:多価カルボン酸成分=テレフタル酸66mol%、イソフタル酸10mol%、アジピン酸24mol%、多価アルコール成分=1,4-ブタンジオール100mol%
物性値:質量平均分子量=50,000、Tg=-6℃、Tm=167℃、ΔHm=23.7J/g [Polyester resin (A) -2]
Product name: Byron GA-1300 manufactured by Toyobo Co., Ltd.
Composition: polycarboxylic acid component = terephthalic acid 66 mol%, isophthalic acid 10 mol%, adipic acid 24 mol%, polyhydric alcohol component = 1,4-butanediol 100 mol%
Physical property values: mass average molecular weight = 50,000, Tg = −6 ° C., Tm = 167 ° C., ΔHm = 23.7 J / g
製品名:東洋紡績社製バイロンGA-1310
組成:多価カルボン酸成分=テレフタル酸71mol%、イソフタル酸29mol%、多価アルコール成分=1,4-ブタンジオール=100mol%
物性値:質量平均分子量=56,000、Tg=27℃、Tm=179℃、ΔHm=24.5J/g [Polyester resin (A) -3]
Product name: Byron GA-1310 manufactured by Toyobo Co., Ltd.
Composition: polyvalent carboxylic acid component = 71 mol% terephthalic acid, 29 mol% isophthalic acid, polyhydric alcohol component = 1,4-butanediol = 100 mol%
Physical property values: mass average molecular weight = 56,000, Tg = 27 ° C., Tm = 179 ° C., ΔHm = 24.5 J / g
製品名:東洋紡績社製バイロン30P
組成:多価カルボン酸成分=テレフタル酸54mol%、セバシン酸46mol%、多価アルコール成分=1,4-ブタンジオール82mol%、エチレングリコール=18mol%
物性値:質量平均分子量=96,000、Tg=-28℃、Tm=125℃、ΔHm=2.0J/g [Polyester resin (B) -1]
Product name: Byron 30P manufactured by Toyobo Co., Ltd.
Composition: polycarboxylic acid component = terephthalic acid 54 mol%, sebacic acid 46 mol%, polyhydric alcohol component = 1,4-butanediol 82 mol%, ethylene glycol = 18 mol%
Physical property values: mass average molecular weight = 96,000, Tg = −28 ° C., Tm = 125 ° C., ΔHm = 2.0 J / g
製品名:東洋紡績社製バイロンバイロンGM-913
組成:多価カルボン酸成分=テレフタル酸66mol%、イソフタル酸34mol%、多価アルコール成分=1,4-ブタンジオール82mol%、ポリテトラメチレンエーテルグリコール18mol%
物性値:質量平均分子量=100,000、Tg=-70℃、Tm=126℃、ΔHm=10.2J/g [Polyester resin (B) -2]
Product name: Byron Byron GM-913 manufactured by Toyobo Co., Ltd.
Composition: polycarboxylic acid component = terephthalic acid 66 mol%, isophthalic acid 34 mol%, polyhydric alcohol component = 12,4-butanediol 82 mol%, polytetramethylene ether glycol 18 mol%
Physical property values: mass average molecular weight = 100,000, Tg = −70 ° C., Tm = 126 ° C., ΔHm = 10.2 J / g
日産化学工業社製微粉メラミン(平均粒径5μm、表面処理無) [melamine]
Fine melamine produced by Nissan Chemical Industries (average particle size 5μm, no surface treatment)
ポリエステル系樹脂(A)-1、及び、微粉メラミンを混合質量比80:20でドライブレンドした後、40mmφ同方向二軸押出機を用いて200℃で混練した後、Tダイより押出し、次いで約40℃のキャスティングロールにて急冷し、厚み100μmのシートを作製した。得られたシートについて、難燃性、引張強度、引張伸度、及び、耐熱性の評価を行った。結果を表1に示す。 Example 1-1
The polyester resin (A) -1 and fine melamine were dry blended at a mixing mass ratio of 80:20, kneaded at 200 ° C. using a 40 mmφ co-directional twin screw extruder, extruded from a T die, and then about The sheet was rapidly cooled with a 40 ° C. casting roll to prepare a sheet having a thickness of 100 μm. The obtained sheet was evaluated for flame retardancy, tensile strength, tensile elongation, and heat resistance. The results are shown in Table 1.
ポリエステル系樹脂(A)-1、及び、微粉メラミンの混合質量比を70:30とした以外は実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 Example 1-2
A sheet having a thickness of 100 μm was produced in the same manner as in Example 1-1 except that the mixing mass ratio of the polyester resin (A) -1 and fine melamine was set to 70:30. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
ポリエステル系樹脂(A)-1、及び、微粉メラミンの混合質量比を50:50とした以外は実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 (Example 1-3)
A sheet having a thickness of 100 μm was produced in the same manner as in Example 1-1 except that the mixing mass ratio of the polyester resin (A) -1 and fine melamine was 50:50. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
ポリエステル系樹脂(A)-2、及び、微粉メラミンを混合質量比70:30でブレンドした後、実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 (Example 1-4)
After blending the polyester resin (A) -2 and fine melamine at a mixing mass ratio of 70:30, a sheet having a thickness of 100 μm was produced in the same manner as in Example 1-1. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
ポリエステル系樹脂(A)-3、及び、微粉メラミンを混合質量比70:30でブレンドした後、実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 (Example 1-5)
After blending the polyester resin (A) -3 and fine melamine at a mixing mass ratio of 70:30, a sheet having a thickness of 100 μm was produced in the same manner as in Example 1-1. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
ポリエステル系樹脂(A)-2、ポリエステル系樹脂(B)-1、及び、微粉メラミンを混合質量比50:20:30でブレンドした後、実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 (Example 1-6)
After blending polyester resin (A) -2, polyester resin (B) -1 and fine melamine at a mixing mass ratio of 50:20:30, a sheet having a thickness of 100 μm is obtained in the same manner as in Example 1-1. Was made. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
ポリエステル系樹脂(A)-2、ポリエステル系樹脂(B)-1、及び、微粉メラミンを混合質量比40:30:30でブレンドした後、実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 (Example 1-7)
After blending polyester resin (A) -2, polyester resin (B) -1 and fine melamine at a mixing mass ratio of 40:30:30, a sheet having a thickness of 100 μm is obtained in the same manner as in Example 1-1. Was made. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
ポリエステル系樹脂(A)-2、ポリエステル系樹脂(B)-1、及び、微粉メラミンを混合質量比30:40:30でブレンドした後、実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 (Example 1-8)
After blending polyester resin (A) -2, polyester resin (B) -1 and fine melamine at a mixing mass ratio of 30:40:30, a sheet having a thickness of 100 μm is obtained in the same manner as in Example 1-1. Was made. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
ポリエステル系樹脂(A)-2、ポリエステル系樹脂(B)-2、及び、微粉メラミンを混合質量比40:30:30でブレンドした後、実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 (Example 1-9)
After blending polyester resin (A) -2, polyester resin (B) -2, and finely divided melamine at a mixing mass ratio of 40:30:30, a sheet having a thickness of 100 μm is obtained in the same manner as in Example 1-1. Was made. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
ポリエステル系樹脂(A)-1、及び、微粉メラミンを混合質量比90:10でブレンドした後、実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 (Comparative Example 1-1)
After blending the polyester resin (A) -1 and fine melamine at a mixing mass ratio of 90:10, a sheet having a thickness of 100 μm was produced in the same manner as in Example 1-1. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
ポリエステル系樹脂(A)-1、及び、微粉メラミンを混合質量比30:70でブレンドした後、実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 (Comparative Example 1-2)
After blending the polyester resin (A) -1 and fine melamine at a mixing mass ratio of 30:70, a sheet having a thickness of 100 μm was produced in the same manner as in Example 1-1. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
ポリエステル系樹脂(B)-2、及び、微粉メラミンを、混合質量比70:30でブレンドした後、実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 (Comparative Example 1-3)
After blending polyester resin (B) -2 and finely divided melamine at a mixing mass ratio of 70:30, a sheet having a thickness of 100 μm was produced in the same manner as in Example 1-1. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
メラミンの代わりに、日産化学工業社製PHOSMEL-200(ポリリン酸メラミン)を用いて、ポリエステル系樹脂(A)-1、及び、PHOSMEL-200を混合質量比70:30でブレンドした後、実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 (Comparative Example 1-4)
After blending polyester resin (A) -1 and PHOSMEL-200 at a mixing mass ratio of 70:30 using PHOSMEL-200 (melamine polyphosphate) manufactured by Nissan Chemical Industries, Ltd. instead of melamine, Example A sheet having a thickness of 100 μm was produced in the same manner as in 1-1. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
メラミンの代わりに、日産化学工業社製MC-860(メラミンシアヌレート)を用いて、ポリエステル系樹脂(A)-1、及び、MC-860を混合質量比70:30でブレンドした後、実施例1-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例1-1と同様の評価を行った結果を表1に示す。 (Comparative Example 1-5)
Example 1 After blending polyester resin (A) -1 and MC-860 at a mixing mass ratio of 70:30 using MC-860 (melamine cyanurate) manufactured by Nissan Chemical Industries, Ltd. instead of melamine A sheet having a thickness of 100 μm was produced in the same manner as in 1-1. Table 1 shows the results of evaluation similar to Example 1-1 for the obtained sheet.
ガラス転移温度Tgが-20℃~40℃であり、結晶融解温度Tmが140℃~190℃であるポリエステル系樹脂(A)と、メラミンとを混合して得られる難燃性ポリエステル系樹脂組成物において、難燃性ポリエステル系樹脂組成物中のメラミンの割合が20~60質量%であるものは、難燃性、引張強度、引張伸度、及び、耐熱性のいずれも合格評価を得ることができることが分かった。 (Discussion)
Flame retardant polyester resin composition obtained by mixing polyester resin (A) having a glass transition temperature Tg of −20 ° C. to 40 ° C. and a crystal melting temperature Tm of 140 ° C. to 190 ° C. with melamine In the case where the ratio of melamine in the flame retardant polyester resin composition is 20 to 60% by mass, the flame retardant property, the tensile strength, the tensile elongation, and the heat resistance can all be evaluated as acceptable. I understood that I could do it.
メラミンは、一般的には難燃剤として用いることは困難であるが、特定のポリエステル系樹脂には難燃剤として用いることができることが分かった。
メラミンの割合は、難燃性ポリエステル系樹脂組成物の20~60質量%であるのが好ましいことが分かった。 In addition, melamine can be made flame retardant by blending it with polyester resin (A), whereas melamine derivatives such as melamine cyanurate and melamine polyphosphate are specific polyester resins (A). The result that can not be flame retardant.
Melamine is generally difficult to use as a flame retardant, but it has been found that it can be used as a flame retardant for certain polyester resins.
It has been found that the proportion of melamine is preferably 20 to 60% by mass of the flame retardant polyester resin composition.
次に、第2の実施形態に係る実施例及び比較例について説明する。 [Example and Comparative Example of Second Embodiment]
Next, examples and comparative examples according to the second embodiment will be described.
厚みが200μm以下の場合は、長さ200mm×幅50mm(厚みはそれぞれの試験片により異なる)の評価用サンプル、厚みが200μmを超える場合は、長さ127mm×幅13mm(厚みはそれぞれの試験片により異なる)の評価用サンプルを用いて、Underwriters Laboratories社の安全標準UL94薄手材料垂直燃焼試験(サンプル厚みが200μm以下の場合)、及び、UL94垂直燃焼試験(サンプル厚みが200μmを超える場合)の手順に基づき、試験回数5回にて燃焼試験を実施し、燃焼の様子(特に燃焼中における滴下物の有無)を観察すると共に燃焼時間(試験回数5回の合計燃焼時間)を測定した。
UL94垂直燃焼試験において、厚みが200μm以下のサンプルについては、UL94VTMの判定基準に基づき、VTM-0、1、2の規格を満たすか否か判例し、VTM-2を満たさないものは規格外と評価し、VTM-0を満たすものを合格品と評価した。また、厚みが200μmを超えるサンプルについては、UL94Vの判定基準に基づき、VTM-0、1、2の規格を満たすか否か判例し、VTM-2を満たさないものは規格外と評価し、VTM-0を満たすものを合格品と評価した。 (1) Flame retardance When the thickness is 200 μm or less, the sample for evaluation of length 200 mm × width 50 mm (thickness varies depending on each test piece), when the thickness exceeds 200 μm, length 127 mm × width 13 mm ( Underwriters Laboratories safety standard UL94 thin material vertical combustion test (when sample thickness is 200 μm or less) and UL94 vertical combustion test (sample thickness is 200 μm) Based on the above procedure, a combustion test is performed at a test count of 5 times, the state of combustion (especially the presence or absence of drops during combustion) is observed, and the combustion time (total combustion time of the test count of 5 times) Was measured.
In the UL94 vertical combustion test, samples with a thickness of 200 μm or less are judged on the basis of the UL94VTM criteria whether or not the VTM-0, 1 and 2 standards are satisfied. A product satisfying VTM-0 was evaluated as an acceptable product. For samples with a thickness exceeding 200 μm, whether or not the standards of VTM-0, 1 and 2 are satisfied is judged based on the UL94V criteria, and those not satisfying VTM-2 are evaluated as nonstandard. Those satisfying −0 were evaluated as acceptable products.
長さ200mm×幅20mm(厚みはそれぞれの試験片により異なる)の評価用サンプルを用いて、JIS C 2318に基づき、引張破断強度、引張破断伸度の測定を行った。破断時の強度と伸びを測定しn=5での平均値を求めた。雰囲気温度23℃、相対湿度50%、引張り速度200mm/min、つかみ間隔100mmにて測定を行い、破断時の強度と伸度を測定し、n=5での平均値を求めた。
引張強度は10MPa以上、引張伸度は10%以上を合格と評価した。 (2) Tensile strength and tensile elongation Using a sample for evaluation of length 200 mm × width 20 mm (thickness varies depending on each test piece), measurement of tensile strength and elongation at break based on JIS C 2318 went. The strength and elongation at break were measured, and the average value at n = 5 was determined. Measurement was performed at an ambient temperature of 23 ° C., a relative humidity of 50%, a pulling speed of 200 mm / min, and a gripping interval of 100 mm, and the strength and elongation at break were measured, and the average value at n = 5 was obtained.
A tensile strength of 10 MPa or more and a tensile elongation of 10% or more were evaluated as acceptable.
長さ200mm×幅20mm(厚みはそれぞれの試験片により異なる)の評価用サンプルを用いて、JIS C 2318に基づき、雰囲気温度23℃、相対湿度50%、引張り速度200mm/min、つかみ間隔100mmにて、つかみ間隔を基準として10%引張った時の応力(I)と、そのままの状態で5分間保持した後の応力(II)から、{(I)-(II)/(I)}×100(%)の式により応力緩和率を測定した。
応力緩和率は50%以上のものを合格と評価した。なお、10%引張った時にサンプルが破断したものについては測定不可と評価した。 (3) Stress relaxation characteristics Using an evaluation sample having a length of 200 mm × width of 20 mm (thickness varies depending on each test piece), based on JIS C 2318, the ambient temperature is 23 ° C., the relative humidity is 50%, and the tensile speed is 200 mm / From (1)-(II) / (II) / (II) / (II), the stress (I) when pulled by 10% based on the gripping interval at the gripping interval of 100 mm and the stress (II) after holding for 5 minutes The stress relaxation rate was measured by the formula (I)} × 100 (%).
A stress relaxation rate of 50% or more was evaluated as acceptable. In addition, about what fractured | ruptured the sample when it pulled 10%, it evaluated that it was unmeasurable.
第1の実施形態に係る実施例と同様に測定及び評価を行った。 (4) Calorie heat of fusion Measurement and evaluation were performed in the same manner as in the example according to the first embodiment.
次に、実施例・比較例で用いた原料、すなわちポリエステル系樹脂(A)、メラミン、ポリエステル系樹脂(B)について説明する。 <Raw material>
Next, the raw materials used in Examples and Comparative Examples, that is, polyester resin (A), melamine, and polyester resin (B) will be described.
製品名:東洋紡績社製バイロンGA-1300
組成:多価カルボン酸成分=テレフタル酸66mol%、イソフタル酸10mol%、アジピン酸24mol%、多価アルコール成分=1,4-ブタンジオール100mol% 物性値:質量平均分子量=50,000、Tg=-6℃、Tm=167℃、ΔHm=23.7J/g [Polyester resin (A) -1]
Product name: Byron GA-1300 manufactured by Toyobo Co., Ltd.
Composition: polycarboxylic acid component = terephthalic acid 66 mol%, isophthalic acid 10 mol%, adipic acid 24 mol%, polyhydric alcohol component = 1,4-butanediol 100 mol% Physical properties: mass average molecular weight = 50,000, Tg = − 6 ° C., Tm = 167 ° C., ΔHm = 23.7 J / g
製品名:東洋紡績社製バイロンGA-1310
組成:多価カルボン酸成分=テレフタル酸71mol%、イソフタル酸29mol%、多価アルコール成分=1,4-ブタンジオール=100mol%
物性値:質量平均分子量=56,000、Tg=27℃、Tm=179℃、ΔHm=24.5J/g [Polyester resin (A) -2]
Product name: Byron GA-1310 manufactured by Toyobo Co., Ltd.
Composition: polyvalent carboxylic acid component = 71 mol% terephthalic acid, 29 mol% isophthalic acid, polyhydric alcohol component = 1,4-butanediol = 100 mol%
Physical property values: mass average molecular weight = 56,000, Tg = 27 ° C., Tm = 179 ° C., ΔHm = 24.5 J / g
製品名:東洋紡績社製バイロン30P
組成:多価カルボン酸成分=テレフタル酸54mol%、セバシン酸46mol%、多価アルコール成分=1,4-ブタンジオール82mol%、エチレングリコール=18mol%
物性値:質量平均分子量=96,000、Tg=-28℃、Tm=125℃、ΔHm=2.0J/g [Polyester resin (A) -3]
Product name: Byron 30P manufactured by Toyobo Co., Ltd.
Composition: polycarboxylic acid component = terephthalic acid 54 mol%, sebacic acid 46 mol%, polyhydric alcohol component = 1,4-butanediol 82 mol%, ethylene glycol = 18 mol%
Physical property values: mass average molecular weight = 96,000, Tg = −28 ° C., Tm = 125 ° C., ΔHm = 2.0 J / g
製品名:日本合成化学工業社製ポリエスターSP160
組成:多価カルボン酸成分=テレフタル酸=62mol%、アジピン酸=19mol%、セバシン酸=19mol%、多価アルコール成分=1,4-ブタンジオール=100mol%、
物性値:質量平均分子量=82,000、Tg=-20℃、Tm=150℃、ΔHm=26.0J/g [Polyester resin (A) -4]
Product name: Polyester SP160 manufactured by Nippon Synthetic Chemical Industry Co., Ltd.
Composition: polycarboxylic acid component = terephthalic acid = 62 mol%, adipic acid = 19 mol%, sebacic acid = 19 mol%, polyhydric alcohol component = 1,4-butanediol = 100 mol%,
Physical property values: mass average molecular weight = 82,000, Tg = −20 ° C., Tm = 150 ° C., ΔHm = 26.0 J / g
製品名:東洋紡績社製バイロンGM-470
組成:多価カルボン酸成分=テレフタル酸86mol%、アジピン酸14mol%、多価アルコール成分=1,4-ブタンジオール87mol%、1,6-ヘプタンジオール13mol%
物性値:質量平均分子量=58,000、Tg=20℃、Tm=185℃、ΔHm=27.0J/g [Polyester resin (A) -5]
Product name: Byron GM-470 manufactured by Toyobo Co., Ltd.
Composition: polyvalent carboxylic acid component = terephthalic acid 86 mol%, adipic acid 14 mol%, polyhydric alcohol component = 1,4-butanediol 87 mol%, 1,6-heptanediol 13 mol%
Physical property values: mass average molecular weight = 58,000, Tg = 20 ° C., Tm = 185 ° C., ΔHm = 27.0 J / g
製品名:東洋紡績社製ペルプレンP40B
組成:多価カルボン酸成分=テレフタル酸=100mol%、多価アルコール成分=1,4-ブタンジオール73mol%、ポリテトラメチレンエーテルグリコール27mol%
物性値:質量平均分子量=148,000、Tg=-70℃、Tm=180℃、ΔHm=2.3J/g [Polyester resin (A) -6]
Product name: Peroprene P40B manufactured by Toyobo Co., Ltd.
Composition: Polycarboxylic acid component = terephthalic acid = 100 mol%, polyhydric alcohol component = 1,4-butanediol 73 mol%, polytetramethylene ether glycol 27 mol%
Physical property values: mass average molecular weight = 148,000, Tg = −70 ° C., Tm = 180 ° C., ΔHm = 2.3 J / g
日産化学工業社製微粉メラミン(平均粒径5μm、表面処理無) [Melamine (B) -1]
Fine melamine produced by Nissan Chemical Industries (average particle size 5μm, no surface treatment)
製品名:ジャパンエポキシレジン社製E4275
組成:ビスフェノールA/ビスフェノールF=25mol%/75mol% [Phenoxy resin (C) -1]
Product name: E4275 manufactured by Japan Epoxy Resin Co., Ltd.
Composition: bisphenol A / bisphenol F = 25 mol% / 75 mol%
製品名:ジャパンエポキシレジン社製E1256
組成:ビスフェノールA=100mol% [Phenoxy resin (C) -2]
Product name: Japan Epoxy Resin E1256
Composition: Bisphenol A = 100 mol%
(A)-1、(A)-3、(B)-1、及び、(C)-1を混合質量比55:20:15:5の割合でドライブレンドした後、40mmφ同方向二軸押出機を用いて200℃で混練した後、Tダイより押出し、次いで約40℃のキャスティングロールにて急冷し、厚み100μmのシートを作製した。得られたシートについて、難燃性、引張強度、引張伸度、及び、応力緩和特性の評価を行った。結果を表2に示す。 Example 2-1
(A) -1, (A) -3, (B) -1, and (C) -1 were dry blended at a mixing mass ratio of 55: 20: 15: 5, and then 40 mmφ co-directional twin screw extrusion After kneading at 200 ° C. using a machine, it was extruded from a T-die and then rapidly cooled with a casting roll at about 40 ° C. to produce a sheet having a thickness of 100 μm. The obtained sheet was evaluated for flame retardancy, tensile strength, tensile elongation, and stress relaxation characteristics. The results are shown in Table 2.
ポリエステル系樹脂(A)-1、(A)-3、(B)-1、及び、(C)-1の混合質量比を45:20:30:5とした以外は実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Example 2-2)
Example 2-1 except that the mixing mass ratio of the polyester resins (A) -1, (A) -3, (B) -1 and (C) -1 was 45: 20: 30: 5 A sheet having a thickness of 100 μm was produced in the same manner. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)-1、(A)-3、(B)-1、及び、(C)-1の混合質量比を15:20:55:5とした以外は実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Example 2-3)
Example 2-1 except that the mixing mass ratio of the polyester resins (A) -1, (A) -3, (B) -1 and (C) -1 was 15: 20: 55: 5 A sheet having a thickness of 100 μm was produced in the same manner. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)-2、(A)-3、(B)-1、及び、(C)-1を混合質量比45:20:30:5の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Example 2-4)
After the polyester resins (A) -2, (A) -3, (B) -1 and (C) -1 were dry blended at a mixing mass ratio of 45: 20: 30: 5, Example 2 A sheet having a thickness of 100 μm was produced in the same manner as in -1. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
(A)-3、(B)-1、及び、(C)-1を混合質量比65:30:5の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Example 2-5)
After dry blending (A) -3, (B) -1, and (C) -1 at a mixing mass ratio of 65: 30: 5, a sheet having a thickness of 100 μm is obtained in the same manner as in Example 2-1. Was made. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)-1、(A)-3、(B)-1、及び、(C)-1を混合質量比65:30:5の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Example 2-6)
After dry blending the polyester resins (A) -1, (A) -3, (B) -1 and (C) -1 at a mixing mass ratio of 65: 30: 5, Example 2-1 A sheet having a thickness of 100 μm was produced in the same manner as described above. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)-4、(B)-1、及び、(C)-1を混合質量比65:30:5の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Example 2-7)
After the polyester resins (A) -4, (B) -1 and (C) -1 were dry blended at a mixing mass ratio of 65: 30: 5, the thickness was determined in the same manner as in Example 2-1. A 100 μm sheet was prepared. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)-5、(B)-1、及び、(C)-1を混合質量比65:30:5の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Example 2-8)
After the polyester resins (A) -5, (B) -1 and (C) -1 were dry blended at a mixing mass ratio of 65: 30: 5, the thickness was determined in the same manner as in Example 2-1. A 100 μm sheet was prepared. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)-1、(A)-3、(B)-1、及び、(C)-1を混合質量比48:20:30:2の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Example 2-9)
After the polyester resins (A) -1, (A) -3, (B) -1 and (C) -1 were dry blended at a mixing mass ratio of 48: 20: 30: 2, Example 2 A sheet having a thickness of 100 μm was produced in the same manner as in -1. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)-1、(A)-3、(B)-1、及び、(C)-1を混合質量比40:20:30:10の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Example 2-10)
Example 2 After dry blending polyester resins (A) -1, (A) -3, (B) -1 and (C) -1 at a mixing mass ratio of 40: 20: 30: 10, Example 2 A sheet having a thickness of 100 μm was produced in the same manner as in -1. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)-1、(A)-3、(B)-1、及び、(C)-1を混合質量比30:20:30:20の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Example 2-11)
Example 2 After dry blending polyester resins (A) -1, (A) -3, (B) -1 and (C) -1 at a mixing mass ratio of 30: 20: 30: 20, Example 2 A sheet having a thickness of 100 μm was produced in the same manner as in -1. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)-1、(A)-3、(B)-1、及び、(C)-2を混合質量比40:20:30:10の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Example 2-12)
After the polyester resins (A) -1, (A) -3, (B) -1 and (C) -2 were dry blended at a mixing mass ratio of 40: 20: 30: 10, Example 2 A sheet having a thickness of 100 μm was produced in the same manner as in -1. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
実施例2-2と同様に、ポリエステル系樹脂(A)-1、(A)-3、(B)-1及び(C)-1を45:20:30:5の混合質量比で配合し、三菱重工製40mmφ小型同方向二軸押出機を用いて190℃でコンパウンドし、ペレット形状にした。得られたペレットを東芝機械製射出成形機 IS50E(スクリュー径25mm)を用い、長さ250mm×幅200mm×厚さ1mmの板材を射出成形した。主な成形条件は以下の通りである。
1)温度条件:シリンダー温度(190℃) 金型温度(30℃)
2)射出条件:射出圧力(115MPa) 保持圧力(55MPa)
3)計量条件:スクリュー回転数(65rpm) 背圧(15MPa)
得られた成形品から評価用サンプルを切り出し、実施例2-1と同様の評価を行った結果を表2に示す。 (Example 2-13)
As in Example 2-2, polyester resins (A) -1, (A) -3, (B) -1 and (C) -1 were blended at a mixing mass ratio of 45: 20: 30: 5. It was compounded at 190 ° C. using a 40 mmφ small-size co-directional twin screw extruder manufactured by Mitsubishi Heavy Industries, and formed into a pellet shape. A plate material having a length of 250 mm, a width of 200 mm and a thickness of 1 mm was injection molded from the obtained pellets using an injection molding machine IS50E (screw diameter: 25 mm) manufactured by Toshiba Machine. The main molding conditions are as follows.
1) Temperature conditions: Cylinder temperature (190 ° C) Mold temperature (30 ° C)
2) Injection conditions: Injection pressure (115 MPa) Holding pressure (55 MPa)
3) Measurement conditions: Screw rotation speed (65 rpm) Back pressure (15 MPa)
Table 2 shows the results obtained by cutting out samples for evaluation from the obtained molded products and performing the same evaluation as in Example 2-1.
ポリエステル系樹脂(A)-1、(A)-3、及び、(B)-1を混合質量比50:20:30の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Comparative Example 2-1)
After the polyester resins (A) -1, (A) -3, and (B) -1 were dry blended at a mixing mass ratio of 50:20:30, the thickness was determined in the same manner as in Example 2-1. A 100 μm sheet was prepared. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)-1、(A)-3、(B)-1、及び、(C)-1を混合質量比70:20:5:5の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Comparative Example 2-2)
The polyester resins (A) -1, (A) -3, (B) -1 and (C) -1 were dry blended at a mixing mass ratio of 70: 20: 5: 5, and then Example 2 A sheet having a thickness of 100 μm was produced in the same manner as in -1. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)-1、(B)-1、及び、(C)-1を混合質量比35:25:40の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Comparative Example 2-3)
After the polyester resins (A) -1, (B) -1 and (C) -1 were dry blended at a mixing mass ratio of 35:25:40, the thickness was determined in the same manner as in Example 2-1. A 100 μm sheet was prepared. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)-1、(B)-1、及び、(C)-1を混合質量比25:70:5の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Comparative Example 2-4)
After the polyester resins (A) -1, (B) -1 and (C) -1 were dry blended at a mixing mass ratio of 25: 70: 5, the thickness was determined in the same manner as in Example 2-1. A 100 μm sheet was prepared. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
メラミンの代わりに日産化学工業社製MC-860(メラミンシアヌレート)を用い、ポリエステル系樹脂(A)-1、(A)-3、(C)-1、及び、MC-860を混合質量比45:20:5:30の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Comparative Example 2-5)
MC-860 (melamine cyanurate) manufactured by Nissan Chemical Industries, Ltd. was used instead of melamine, and the polyester resins (A) -1, (A) -3, (C) -1 and MC-860 were mixed in a mass ratio. After dry blending at a ratio of 45: 20: 5: 30, a sheet having a thickness of 100 μm was produced in the same manner as in Example 2-1. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
メラミンの代わりに昭和電工社製H42S(ステアリン酸処理水酸化アルミニウム)を用い、(A)-1、(A)-3、(C)-1、及び、H42Sを混合質量比45:20:5:30の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Comparative Example 2-6)
Instead of melamine, H42S (stearic acid-treated aluminum hydroxide) manufactured by Showa Denko KK was used, and (A) -1, (A) -3, (C) -1, and H42S were mixed at a mass ratio of 45: 20: 5. : After dry blending at a ratio of 30, a sheet having a thickness of 100 μm was produced in the same manner as in Example 2-1. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
ポリエステル系樹脂(A)の代わりに、ポリエステル系樹脂(A)-6(ペルプレンP40B)を用い、(A)-6、(B)-1、及び、(C)-1を混合質量比65:25:10の割合でドライブレンドした後、実施例2-1と同様の方法で厚み100μmのシートを作製した。得られたシートに関して実施例2-1と同様の評価を行った結果を表2に示す。 (Comparative Example 2-7)
Instead of the polyester resin (A), a polyester resin (A) -6 (Perprene P40B) is used, and (A) -6, (B) -1 and (C) -1 are mixed at a mass ratio of 65: After dry blending at a ratio of 25:10, a sheet having a thickness of 100 μm was produced in the same manner as in Example 2-1. Table 2 shows the results of evaluation similar to Example 2-1 for the obtained sheet.
フェノキシ樹脂(C)の割合は、難燃性ポリエステル系樹脂組成物の1~25質量%あるのが好ましく、特に2質量%以上、中でも5質量%以上であるのがさらに好ましく、20質量%以下、中でも10質量%以下であるのがさらに好ましいことが分かった。 It is confirmed that the stress relaxation property of the polyester resin (A) can be improved by adding the phenoxy resin (C) to the polyester resin (A), and the flame retardancy can be further improved. did it.
The proportion of the phenoxy resin (C) is preferably 1 to 25% by mass of the flame retardant polyester resin composition, particularly 2% by mass or more, more preferably 5% by mass or more, and more preferably 20% by mass or less. In particular, it was found that the content is more preferably 10% by mass or less.
メラミンは、一般的には難燃剤として用いることは困難であるが、特定のポリエステル系樹脂には難燃剤として用いることができることが分かった。すなわち、表2の結果より、ポリエステル系樹脂(A)-6に対しては難燃剤として機能しない一方、ポリエステル系樹脂(A)-1~(A)-5に対しては難燃剤として機能することが分かった。
メラミン(B)の割合は、難燃性ポリエステル系樹脂組成物の10~60質量%であるのが好ましく、特に20質量%以上、中でも30質量%以上であるのがさらに好ましく、50質量%以下、中でも40質量%以下であるのがさらに好ましいことが分かった。 In addition, melamine can be made flame retardant by blending it with polyester resin (A), whereas melamine derivatives such as melamine cyanurate and melamine polyphosphate are specific polyester resins (A). The result that can not be flame retardant.
Melamine is generally difficult to use as a flame retardant, but it has been found that it can be used as a flame retardant for certain polyester resins. That is, from the results in Table 2, it does not function as a flame retardant for the polyester resin (A) -6, but functions as a flame retardant for the polyester resins (A) -1 to (A) -5. I understood that.
The proportion of melamine (B) is preferably 10 to 60% by mass of the flame retardant polyester resin composition, particularly 20% by mass or more, more preferably 30% by mass or more, and more preferably 50% by mass or less. In particular, it was found that 40% by mass or less is more preferable.
先ず、第3の実施形態に係る実施例及び比較例について説明する。
下記実施例中に示す結果は以下の方法で評価を行った。 [Example and Comparative Example of Third Embodiment]
First, examples and comparative examples according to the third embodiment will be described.
The results shown in the following examples were evaluated by the following methods.
<UL94VTM>
難燃性積層体の難燃性の評価は、以下のようにUL94垂直燃焼試験により評価を行なった。すなわち、長さ200mm×幅50mm(厚みはそれぞれの試験片により異なる)の評価用サンプルを用いて、Underwriters Laboratories社の安全標準UL94垂直燃焼試験の手順に基づき、試験回数5回にて燃焼試験を実施した。UL94垂直燃焼試験UL94VTMの判定基準に基づき、VTM-0規格を満たす積層体を合格とした。 (1) Flame retardancy <UL94VTM>
The flame retardancy of the flame retardant laminate was evaluated by the UL94 vertical combustion test as follows. That is, using a sample for evaluation having a length of 200 mm × width of 50 mm (thickness varies depending on each test piece), a combustion test was performed with 5 tests based on the safety standard UL94 vertical combustion test procedure of Underwriters Laboratories. Carried out. Based on the criteria of UL94 vertical combustion test UL94VTM, a laminate satisfying the VTM-0 standard was accepted.
前記UL94VTM試験において、燃焼時間を以下の手順に従って評価した。
先ず、バーナーの炎の長さが20mm±1mmとなるように調整し、試験積層体に炎が10mm±1mm接するようにして、所定の時間接炎した。
次に、前記バーナーの炎を試験積層体から外し、試験積層体の燃焼時間をt1とした。
次に、前記での燃焼時間終了後、所定の時間、前記と同様の方法で接炎した。
次に、前記での接煙を外した後の、試験積層体の燃料時間をt2とし、さらに試験積層体の無煙燃焼時間をt3とした。 <Burning time>
In the UL94VTM test, the burning time was evaluated according to the following procedure.
First, the flame length of the burner was adjusted so as to be 20 mm ± 1 mm, and the flame was in contact with the test laminate for 10 mm ± 1 mm for a predetermined time.
Next, the flame of the burner was removed from the test laminate, and the burning time of the test laminate was t1.
Next, after completion of the burning time described above, flame contact was performed in the same manner as described above for a predetermined time.
Next, the fuel time of the test laminate after removing the smoke contact described above was t2, and the smokeless combustion time of the test laminate was t3.
剥離強度は、引張試験機(株式会社インテスコ製:恒温槽付き材料試験器201X)を用いて、A層およびB層間の剥離強度を測定した。測定方法は、T型はく離試験により測定を行なった(JISK6854-3 1999)。評価用サンプル10mm幅のものを使用し、雰囲気温度23℃、剥離速度10mm/分でT型剥離試験を実施した。剥離強度は4N/10mm以上を合格とした。 (2) Peel strength Peel strength was measured by using a tensile tester (manufactured by Intesco Corporation: material tester 201X with a thermostatic bath) to measure the peel strength between the A layer and the B layer. The measurement was carried out by a T-type peeling test (JIS K6854-3 1999). An evaluation sample having a width of 10 mm was used, and a T-type peel test was performed at an atmospheric temperature of 23 ° C. and a peel rate of 10 mm / min. The peel strength was 4N / 10 mm or more as acceptable.
長さ200mm×幅15mm(厚みはそれぞれの試験片により異なる)の評価用サンプルを用いて、JIS C 2318に基づき、引張破断強度、引張破断伸度の測定を行った。破断時の強度と伸びを測定しn=5での平均値を求めた。雰囲気温度23℃、相対湿度50%、引張り速度100mm/min、つかみ間隔100mmにて測定を行い、破断時の強度と伸度を測定し、n=5での平均値を求めた。引張強度は80MPa以上、引張伸度は50%以上を合格とした。 (3) Tensile strength and tensile elongation Using a sample for evaluation having a length of 200 mm x a width of 15 mm (thickness varies depending on each test piece), the tensile strength at break and the tensile elongation at break were measured based on JIS C 2318. went. The strength and elongation at break were measured, and the average value at n = 5 was determined. Measurement was performed at an ambient temperature of 23 ° C., a relative humidity of 50%, a pulling speed of 100 mm / min, and a gripping interval of 100 mm, and the strength and elongation at break were measured, and the average value at n = 5 was obtained. The tensile strength was 80 MPa or more, and the tensile elongation was 50% or more.
長さ100mm×幅100mm(厚みはそれぞれの試験片により異なる)の評価用サンプルをベーキング試験装置(大栄科学精器製作所製DKS-5S)内に静置し、100℃で15分間加熱した。加熱後のサンプルの外観を目視にて観察し、加熱前と変化がないものを○、収縮、シワ、変形等が生じているものを×とした。 (4) Heat resistance A sample for evaluation having a length of 100 mm × width of 100 mm (thickness varies depending on each test piece) is allowed to stand in a baking test apparatus (DKS-5S manufactured by Daiei Kagaku Seisakusho Co., Ltd.). Heated for minutes. The external appearance of the sample after heating was visually observed, and the sample that did not change from that before heating was evaluated as “◯”, and the sample that caused shrinkage, wrinkles, deformation, etc. was evaluated as “X”.
「B層-A」
ポリエステル系樹脂として三菱化学社製ノバペックス(登録商標)(ポリエチレンテレフタレート、IV:0.65、ΔHm=55J/g)を用い、先ず、ノバペックスを40mm直径単軸押出機にて260℃で混練した後、口金から押出し、次いで約40℃のキャスティングロールにて急冷し、厚さ225μmの非晶シートを作製した。次いで、三菱重工株式会社製逐次2軸テンターに通紙し、95℃でMD(長手方向)に延伸倍率で3倍に延伸を行い、続いて、110℃でTD(横手方向)に延伸倍率で3倍に延伸を行った。さらにその後、160℃で15秒熱処理を行い、厚さ25μmの二軸延伸フィルムを得た。 <Preparation of B layer>
"B layer-A"
After using NOVAPEX (registered trademark) (polyethylene terephthalate, IV: 0.65, ΔHm = 55 J / g) manufactured by Mitsubishi Chemical Corporation as the polyester resin, NOVAPEX was first kneaded at 260 ° C. with a 40 mm diameter single screw extruder. Then, it was extruded from the die, and then rapidly cooled with a casting roll at about 40 ° C. to produce an amorphous sheet having a thickness of 225 μm. Next, the paper is passed through a sequential biaxial tenter manufactured by Mitsubishi Heavy Industries, Ltd., stretched at 95 ° C. in the MD (longitudinal direction) at a stretch ratio of 3 times, and subsequently at 110 ° C. in the TD (transverse direction) at the stretch ratio. The film was stretched 3 times. Thereafter, a heat treatment was performed at 160 ° C. for 15 seconds to obtain a biaxially stretched film having a thickness of 25 μm.
ポリエステルフィルムAと同様の方法、条件で厚さ108μmの非晶シートを作製した後、ポリエステルフィルムAと同様の方法、条件で延伸を行い、厚さ12μmの二軸延伸フィルムを得た。 "B layer-B"
An amorphous sheet having a thickness of 108 μm was prepared under the same method and conditions as the polyester film A, and then stretched under the same methods and conditions as the polyester film A to obtain a biaxially stretched film having a thickness of 12 μm.
ポリエステル系樹脂としてイーストマンケミカル社製coplyester6763(ポリエチレンテレフタレートグリコール、ガラス転移温度=81℃、ΔHm=0J/gを用い、coplyester6763を40mm直径単軸押出機にて260℃で混練した後、口金から押出し、次いで約40℃のキャスティングロールにて急冷し、厚さ25μmの非晶シートを作製した。 "B layer-C"
As polyester-based resin, Eastman Chemical Co., Ltd., copyester 6763 (polyethylene terephthalate glycol, glass transition temperature = 81 ° C., ΔHm = 0 J / g) was used. Then, it was quenched with a casting roll at about 40 ° C. to produce an amorphous sheet having a thickness of 25 μm.
ポリエステル系樹脂(A)として、東洋紡績社製バイロンGM-443(テレフタル酸:26.5mol%、イソフタル酸:19.8mol%、アジピン酸:4.7mol%、1,4-ブタンジオール:50mol%、ガラス転移温度:26℃、結晶融解熱量ΔHm:22.8J/g)、難燃剤として、日産化学社製微粒径メラミン(平均粒径5μm)を用い、バイロンGM-443と微粒径メラミンを混合質量比80:20でドライブレンドした後、40mm直径同方向二軸押出機を用いて200℃で混練し、Tダイより押出すと同時に、B層-Aをキャストロール側から貼り合わせることにより、層構成がA層/B層となる厚さ50μmの積層体(A層=25μm、B層-A=25μm)を得た。得られた積層体について、難燃性、剥離強度、引張強度、及び、引張伸度の評価を行った結果を表3に示す。 Example 3-1
As a polyester resin (A), Byron GM-443 manufactured by Toyobo Co., Ltd. (terephthalic acid: 26.5 mol%, isophthalic acid: 19.8 mol%, adipic acid: 4.7 mol%, 1,4-butanediol: 50 mol% , Glass transition temperature: 26 ° C., heat of crystal melting ΔHm: 22.8 J / g), as a flame retardant, fine particle size melamine (average particle size 5 μm) manufactured by Nissan Chemical Co., Ltd., Byron GM-443 and fine particle size melamine Is dry blended at a mixing mass ratio of 80:20, then kneaded at 200 ° C. using a 40 mm diameter co-axial twin screw extruder, extruded from a T die, and simultaneously layer B-A is bonded from the cast roll side. As a result, a laminated body (A layer = 25 μm, B layer−A = 25 μm) having a layer configuration of A layer / B layer was obtained. Table 3 shows the results of evaluation of flame retardancy, peel strength, tensile strength, and tensile elongation of the obtained laminate.
A層として、バイロンGM-443と微粒径メラミンの混合質量比を60:40とした以外は実施例3-1と同様の方法で厚さ50μm(A層=25μm、B層-A=25μm)の積層体を得た。得られた積層体に関して実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-2)
As the A layer, a thickness of 50 μm (A layer = 25 μm, B layer−A = 25 μm) was obtained in the same manner as in Example 3-1, except that the mixing mass ratio of Byron GM-443 and fine particle size melamine was 60:40. ) Was obtained. Table 3 shows the results of evaluation similar to Example 3-1 for the obtained laminate.
A層として、バイロンGM-443と微粒径メラミンの混合質量比を40:60とした以外は実施例3-1と同様の方法で厚さ50μm(A層=25μm、B層-A層=25μm)の積層体を得た。得られた積層体に関して実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-3)
As the A layer, a thickness of 50 μm (A layer = 25 μm, B layer−A layer = with the same method as in Example 3-1 except that the mixing mass ratio of Byron GM-443 and fine particle size melamine was 40:60. 25 μm) was obtained. Table 3 shows the results of evaluation similar to Example 3-1 for the obtained laminate.
A層として、バイロンGM-443と微粒径メラミンの混合質量比を25:75とした以外は実施例3-1と同様の方法で厚さ50μm(A層=25μm、B層-A層=25μm)の積層体を得た。得られた積層体に関して実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-4)
As the A layer, a thickness of 50 μm (A layer = 25 μm, B layer−A layer = the same as in Example 3-1) except that the mixing mass ratio of Byron GM-443 and fine particle size melamine was 25:75. 25 μm) was obtained. Table 3 shows the results of evaluation similar to Example 3-1 for the obtained laminate.
バイロンGM-443と微粒径メラミンを混合質量比60:40でドライブレンドした後、40mm直径同方向二軸押出機を用いて200℃で混練し、Tダイより押出すと同時にB層-Aをキャストロール側とニップロール側から貼り合わせることにより、層構成がB層-A/A層/B層-Aとなる厚さ70μm(A層=20μm、B層-A=25μm)の積層体を得た。得られた積層体について実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-5)
Byron GM-443 and fine particle size melamine were dry blended at a mixing mass ratio of 60:40, then kneaded at 200 ° C. using a 40 mm diameter same-direction twin screw extruder, extruded from a T die, and layer B-A Are laminated from the cast roll side and the nip roll side to form a laminate having a layer configuration of B layer-A / A layer / B layer-A with a thickness of 70 μm (A layer = 20 μm, B layer-A = 25 μm). Obtained. Table 3 shows the results of evaluation similar to that of Example 3-1 for the obtained laminate.
B層-Aの代わりにB層-Bを用いた以外は実施例3-2と同様の方法で厚さ40μm(A層=28μm、B層-B=12μm)の積層体を得た。得られた積層体について実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-6)
A laminate having a thickness of 40 μm (A layer = 28 μm, B layer−B = 12 μm) was obtained in the same manner as in Example 3-2 except that B layer-B was used instead of B layer-A. Table 3 shows the results of evaluation similar to that of Example 3-1 for the obtained laminate.
ポリエステル系樹脂(A)として、東洋紡績社製バイロンGA-1300(テレフタル酸:32.8mol%、イソフタル酸:5.1mol%、アジピン酸:12.1mol%、1,4-ブタンジオール:50mol%、ガラス転移温度=-6℃、ΔHm=23.7J/g)を用いた以外は実施例3-2と同様の方法で厚さ50μm(A層=25μm、B層-A=25μm)の積層体を得た。得られた積層体について実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-7)
Byron GA-1300 manufactured by Toyobo Co., Ltd. (terephthalic acid: 32.8 mol%, isophthalic acid: 5.1 mol%, adipic acid: 12.1 mol%, 1,4-butanediol: 50 mol% as the polyester resin (A) And a glass transition temperature = −6 ° C., ΔHm = 23.7 J / g), and a thickness of 50 μm (A layer = 25 μm, B layer—A = 25 μm) in the same manner as in Example 3-2 Got the body. Table 3 shows the results of evaluation similar to that of Example 3-1 for the obtained laminate.
ポリエステル系樹脂(A)として、東洋紡績社製バイロン30P(テレフタル酸:27.0mol%、イソフタル酸:23.0mol%、エチレングリコール:50mol%、ガラス転移温度=-28℃、ΔHm=9.0J/g)を用いた以外は実施例3-2と同様の方法で厚さ50μm(A層=25μm、B層-A=25μm)の積層体を得た。得られた積層体について実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-8)
Byron 30P manufactured by Toyobo Co., Ltd. (terephthalic acid: 27.0 mol%, isophthalic acid: 23.0 mol%, ethylene glycol: 50 mol%, glass transition temperature = −28 ° C., ΔHm = 9.0 J / G) was used to obtain a laminate having a thickness of 50 μm (A layer = 25 μm, B layer−A = 25 μm) in the same manner as in Example 3-2. Table 3 shows the results of evaluation similar to that of Example 3-1 for the obtained laminate.
A層として、バイロンGM-443、バイロン30P、及び、微粒径メラミンを質量比20:40:40で混合した後、実施例3-1と同様の方法で厚さ50μm(A層=25μm、B層-A層=25μm)の積層体を得た。得られた積層体に関して実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-9)
By mixing Byron GM-443, Byron 30P, and fine particle size melamine at a mass ratio of 20:40:40 as the A layer, the thickness was 50 μm (A layer = 25 μm, A laminate of (B layer−A layer = 25 μm) was obtained. Table 3 shows the results of evaluation similar to Example 3-1 for the obtained laminate.
ポリエステル系樹脂(A)として、三菱化学社製GSPla AD92W(ポリブチレンサクシネート・アジペート共重合体、ガラス転移温度=-40℃、ΔHm=35J/g)を用いた以外は実施例3-2と同様の方法で厚さ50μm(A層=25μm、B層-A=25μm)の積層体を得た。得られた積層体について実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-10)
Example 3-2 except that GSPla AD92W (polybutylene succinate-adipate copolymer, glass transition temperature = −40 ° C., ΔHm = 35 J / g) manufactured by Mitsubishi Chemical Corporation was used as the polyester resin (A). A laminate having a thickness of 50 μm (A layer = 25 μm, B layer−A = 25 μm) was obtained in the same manner. Table 3 shows the results of evaluation similar to that of Example 3-1 for the obtained laminate.
ポリエステル系樹脂(A)として、BASF社製エコフレックスF(ポリブチレンアジペート・テレフタレート共重合体、ガラス転移温度=-30℃、ΔHm=21J/g)を用いた以外は実施例3-2と同様の方法で厚さ50μm(A層=25μm、B層-A=25μm)の積層体を得た。得られた積層体について実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-11)
Example 3-2 except that BASF Ecoflex F (polybutylene adipate-terephthalate copolymer, glass transition temperature = −30 ° C., ΔHm = 21 J / g) was used as the polyester resin (A). In this way, a laminate having a thickness of 50 μm (A layer = 25 μm, B layer−A = 25 μm) was obtained. Table 3 shows the results of evaluation similar to that of Example 3-1 for the obtained laminate.
ポリエステル系樹脂(A)として、三菱化学社製GSPla AD92W(ポリブチレンサクシネート・アジペート共重合体、ΔHm=35J/g)、を同様の方法でを用いた以外は実施例3-1と同様の方法で厚さ50μm(A層=25μm、B層-A=25μm)の積層体を得た。得られた積層体について実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-12)
As the polyester-based resin (A), GSPla AD92W (polybutylene succinate-adipate copolymer, ΔHm = 35 J / g) manufactured by Mitsubishi Chemical Corporation was used in the same manner as in Example 3-1. By the method, a laminate having a thickness of 50 μm (A layer = 25 μm, B layer−A = 25 μm) was obtained. Table 3 shows the results of evaluation similar to that of Example 3-1 for the obtained laminate.
A層として、GSPla AD92Wとメラミンの混合質量比を40:60とした以外は実施例3-1と同様の方法で厚さ50μmの積層体を得た。得られた積層体に関して実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-13)
As a layer A, a laminate having a thickness of 50 μm was obtained in the same manner as in Example 3-1, except that the mixing mass ratio of GSPla AD92W and melamine was set to 40:60. Table 3 shows the results of evaluation similar to Example 3-1 for the obtained laminate.
GSPla AD92Wとメラミンを混合質量比60:40でドライブレンドした後、40mm直径同方向二軸押出機を用いて200℃で混練し、Tダイより押出すと同時に層(B)-Aをキャストロール側とニップロール側から貼り合わせることにより、層構成がB層-A/A層/B層-Aとなる厚さ100μmの積層体を得た。得られた積層体について実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-14)
GSPla AD92W and melamine were dry blended at a mixing mass ratio of 60:40, then kneaded at 200 ° C. using a 40 mm diameter same-direction twin screw extruder, extruded from a T die, and layer (B) -A was cast roll. By laminating from the nip roll side and the nip roll side, a laminate having a layer structure of B layer-A / A layer / B layer-A having a thickness of 100 μm was obtained. Table 3 shows the results of evaluation similar to that of Example 3-1 for the obtained laminate.
B層-Aの代わりにB層-Bを用いた以外は実施例3-2と同様の方法で厚さ50μmの積層体を得た。得られた積層体について実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-15)
A laminate having a thickness of 50 μm was obtained in the same manner as in Example 3-2 except that B layer-B was used instead of B layer-A. Table 3 shows the results of evaluation similar to that of Example 3-1 for the obtained laminate.
B層-Aの代わりにB層-Cを用いた以外は実施例3-2と同様の方法で厚さ50μm(A層=25μm、B層-C=25μm)の積層体を得た。得られた積層体について実施例3-1と同様の評価を行った結果を表3に示す。 (Example 3-16)
A laminate having a thickness of 50 μm (A layer = 25 μm, B layer-C = 25 μm) was obtained in the same manner as in Example 3-2 except that B layer-C was used instead of B layer-A. Table 3 shows the results of evaluation similar to that of Example 3-1 for the obtained laminate.
B層-Aの代わりにB層-Cを用いた以外は実施例3-10と同様の方法で厚さ50μmの積層体を得た。得られた積層体について実施例3-10と同様の評価を行った結果を表3に示す。 (Example 3-17)
A laminate having a thickness of 50 μm was obtained in the same manner as in Example 3-10 except that B layer-C was used instead of B layer-A. Table 3 shows the results of evaluation similar to that of Example 3-10 performed on the obtained laminate.
バイロンGM-443と微粒径メラミンを混合質量比60:40でブレンドした後、実施例3-1と同様の方法で、B層を張り合わせない厚さ50μmのシートを得た。得られた単層体に関して実施例3-1と同様の評価を行った結果を表4に示す。 (Comparative Example 3-1)
Byron GM-443 and fine particle size melamine were blended at a mixing mass ratio of 60:40, and then a sheet having a thickness of 50 μm without layering the layer B was obtained in the same manner as in Example 3-1. Table 4 shows the results of evaluation similar to Example 3-1 for the obtained single-layer body.
A層として、バイロンGM-443と微粒径メラミンの混合質量比を95:5とした以外は実施例3-1と同様の方法で厚さ50μm(A層=25μm、B層-A=25μm)の積層体を得た。得られた積層体に関して実施例3-1と同様の評価を行った結果を表4に示す。 (Comparative Example 3-2)
As the A layer, a thickness of 50 μm (A layer = 25 μm, B layer−A = 25 μm) was obtained in the same manner as in Example 3-1, except that the mixing mass ratio of Byron GM-443 and fine particle size melamine was 95: 5. ) Was obtained. Table 4 shows the results of evaluation similar to Example 3-1 for the obtained laminate.
ポリエステル系樹脂(A)の代わりに、三菱ガス化学社製IUPEC
PEC-350(ポリブチレンサクシネート・カーボネート共重合体、ΔHm=55J/g)を用い、IUPEC PEC-350と微粒径メラミンの混合質量比を60:40でドライブレンドした後、実施例3-1と同様の方法で厚さ50μm(A層=25μm、B層-A=25μm)の積層体を得た。得られた積層体に関して実施例3-1と同様の評価を行った結果を表4に示す。 (Comparative Example 3-3)
IUPEC made by Mitsubishi Gas Chemical Company instead of polyester resin (A)
PEC-350 (polybutylene succinate-carbonate copolymer, ΔHm = 55 J / g) was used and dry blended at a mixing mass ratio of IUPEC PEC-350 and fine particle size melamine of 60:40. 1 to obtain a laminate having a thickness of 50 μm (A layer = 25 μm, B layer−A = 25 μm). Table 4 shows the results of evaluation similar to Example 3-1 for the obtained laminate.
微粒径メラミンの代わりに日産化学工業社製MC-600(メラミンシアヌレート)を用い、バイロンGM-443とMC-601を混合質量比60:40でブレンドした後、実施例3-1と同様の方法で厚さ50μm(A層=25μm、B層-A=25μm)の積層体を得た。得られた積層体に関して実施例3-1と同様の評価を行った結果を表4に示す。 (Comparative Example 3-4)
MC-600 (melamine cyanurate) manufactured by Nissan Chemical Industries, Ltd. was used in place of the fine particle size melamine, and Byron GM-443 and MC-601 were blended at a mixing mass ratio of 60:40, and then the same as in Example 3-1. In this way, a laminate having a thickness of 50 μm (A layer = 25 μm, B layer−A = 25 μm) was obtained. Table 4 shows the results of evaluation similar to Example 3-1 for the obtained laminate.
微粒径メラミンの代わりに日本軽金属社製BF013ST(水酸化アルミニウム)を用い、バイロンGM-443とBF013STを混合質量比60:40でブレンドした後、実施例3-1と同様の方法で厚さ50μm(A層=25μm、B層-A=25μm)の積層体を得た。得られた積層体に関して実施例3-1と同様の評価を行った結果を表4に示す。 (Comparative Example 3-5)
BF013ST (aluminum hydroxide) manufactured by Nippon Light Metal Co., Ltd. was used in place of the fine particle size melamine. Byron GM-443 and BF013ST were blended at a mixing mass ratio of 60:40, and then the thickness was determined in the same manner as in Example 3-1. A laminated body of 50 μm (A layer = 25 μm, B layer−A = 25 μm) was obtained. Table 4 shows the results of evaluation similar to Example 3-1 for the obtained laminate.
GSPla AD92Wと微粒径メラミンを混合質量比60:40でブレンドした後、実施例3-1と同様の方法で、B層を張り合わせない厚さ50μmのシートを得た。得られた単層体に関して実施例3-1と同様の評価を行った結果を表4に示す。 (Comparative Example 3-6)
After blending GSPla AD92W and fine particle size melamine at a mixing mass ratio of 60:40, a sheet having a thickness of 50 μm without layering the layer B was obtained in the same manner as in Example 3-1. Table 4 shows the results of evaluation similar to Example 3-1 for the obtained single-layer body.
A層として、GSPla AD92Wと微粒径メラミンの混合質量比を95:5とした以外は実施例3-1と同様の方法で厚さ50μm(A層=25μm、B層-A=25μm)の積層体を得た。得られた積層体に関して実施例3-1と同様の評価を行った結果を表4に示す。 (Comparative Example 3-7)
A layer having a thickness of 50 μm (A layer = 25 μm, B layer—A = 25 μm) was prepared in the same manner as in Example 3-1, except that the mixing mass ratio of GSPla AD92W and fine particle size melamine was 95: 5. A laminate was obtained. Table 4 shows the results of evaluation similar to Example 3-1 for the obtained laminate.
メラミンの代わりに日産化学工業社製MC-600(メラミンシアヌレート)を用い、GSPla AD92WとMC-600を混合質量比60:40でブレンドした後、実施例3-1と同様の方法で厚さ50μmの積層体を得た。得られた積層体に関して実施例3-1と同様の評価を行った結果を表4に示す。 (Comparative Example 3-8)
MC-600 (melamine cyanurate) manufactured by Nissan Chemical Industries, Ltd. was used instead of melamine, and GSPla AD92W and MC-600 were blended at a mixing mass ratio of 60:40, and then the thickness was determined in the same manner as in Example 3-1. A 50 μm laminate was obtained. Table 4 shows the results of evaluation similar to Example 3-1 for the obtained laminate.
メラミンの代わりに日本軽金属社製BF013ST(水酸化アルミニウム)を用い、GSPla AD92WとBF013STを混合質量比60:40でブレンドした後、実施例3-1と同様の方法で厚さ50μmの積層体を得た。得られた積層体に関して実施例3-1と同様の評価を行った結果を表4に示す。 (Comparative Example 3-9)
BF013ST (aluminum hydroxide) manufactured by Nippon Light Metal Co., Ltd. was used in place of melamine, and GSPla AD92W and BF013ST were blended at a mixing mass ratio of 60:40, and then a 50 μm thick laminate was formed in the same manner as in Example 3-1. Obtained. Table 4 shows the results of evaluation similar to Example 3-1 for the obtained laminate.
次に、第4の実施形態に係る実施例及び比較例について説明する。
実施例中に示す結果は以下の方法で評価を行った。 [Example and Comparative Example of Fourth Embodiment]
Next, examples and comparative examples according to the fourth embodiment will be described.
The results shown in the examples were evaluated by the following methods.
第3の実施形態に係る実施例と同様に測定及び評価した。 (1) Flame retardancy Measurement and evaluation were performed in the same manner as in the example according to the third embodiment.
金属との接着性評価として、図1に示す方法にて、A層と錫メッキ銅箔間の剥離強度測定を行なった。
剥離強度の測定は、引張試験機(株式会社インテスコ製:恒温槽付き材料試験器201X)を用いて行なった。評価用サンプル10mm幅のものを使用し、雰囲気温度-20℃、23℃、及び、80℃、剥離速度10mm/分で180℃剥離試験を実施した。全ての温度で剥離強度が5N/10mm(すなわち5N/cm)以上のものを合格とした。 (2) Adhesiveness with metal As an adhesive evaluation with a metal, the peel strength between the A layer and the tin-plated copper foil was measured by the method shown in FIG.
The peel strength was measured using a tensile tester (manufactured by Intesco Corporation: material tester with thermostat 201X). An evaluation sample having a width of 10 mm was used, and a 180 ° C. peeling test was performed at an atmospheric temperature of −20 ° C., 23 ° C. and 80 ° C., and a peeling speed of 10 mm / min. A film having a peel strength of 5 N / 10 mm (that is, 5 N / cm) or more at all temperatures was accepted.
長さ600mm×幅30mm(厚みはそれぞれの試験片により異なる)の評価用サンプル(フラットケーブル)を、ベーキング試験装置(大栄科学精器製作所製DKS-5S)内に静置し、120℃で24時間加熱した。
加熱後のサンプルの外観を目視にて観察し、銅箔の剥離、フラットケーブルの収縮、シワ、変形等がないものを「○」、銅箔の剥離、フラットケーブルの収縮、シワ、変形等が生じているものを「×」と評価した。 (3) Heat resistance A sample for evaluation (flat cable) having a length of 600 mm × width of 30 mm (thickness varies depending on each test piece) is left in a baking test apparatus (DKS-5S manufactured by Daiei Kagaku Seiki Seisakusho). And heated at 120 ° C. for 24 hours.
Visually observe the appearance of the sample after heating, “○” if there is no copper foil peeling, flat cable shrinkage, wrinkles, deformation, etc., copper foil peeling, flat cable shrinkage, wrinkles, deformation, etc. What was produced was evaluated as “x”.
B層を構成するフィルムとして、次の2種類のフィルム(「B層-A」「B層-B」)を作製し用意した。 <Preparation of layer B>
The following two types of films (“B layer-A” and “B layer-B”) were prepared and prepared as the film constituting the B layer.
ポリエステル系樹脂として三菱化学社製ノバペックス(ポリエチレンテレフタレート、ガラス転移温度=79℃、ΔHm=55J/g)を用い、まず、ノバペックスを40mmφ単軸押出機にて260℃で混練した後、口金から押出し、次いで約40℃のキャスティングロールにて急冷し、厚さ225μmの非晶シートを作製した。次いで、三菱重工株式会社製逐次2軸テンターに通紙し、95℃でMD(長手方向)に延伸倍率で3倍に延伸を行い、続いて、110℃でTD(横手方向)に延伸倍率で3倍に延伸を行った。さらにその後、160℃で15秒熱処理を行い、厚さ25μmの二軸延伸フィルムを得た。 “B layer-A”:
Using Novapex (polyethylene terephthalate, glass transition temperature = 79 ° C., ΔHm = 55 J / g) manufactured by Mitsubishi Chemical Corporation as the polyester-based resin, the Novapex was first kneaded at 260 ° C. with a 40 mmφ single screw extruder and then extruded from the die. Then, it was rapidly cooled with a casting roll at about 40 ° C. to produce an amorphous sheet having a thickness of 225 μm. Next, the paper is passed through a sequential biaxial tenter manufactured by Mitsubishi Heavy Industries, Ltd., stretched at 95 ° C. in the MD (longitudinal direction) at a stretch ratio of 3 times, and subsequently at 110 ° C. in the TD (transverse direction) at the stretch ratio. The film was stretched 3 times. Thereafter, a heat treatment was performed at 160 ° C. for 15 seconds to obtain a biaxially stretched film having a thickness of 25 μm.
ポリエステル系樹脂としてイーストマンケミカル社製coplyester6763(ポリエチレンテレフタレートグリコール、ガラス転移温度=81℃、ΔHm=0J/g)を用い、coplyester6763を40mmφ単軸押出機にて260℃で混練した後、口金から押出し、次いで約40℃のキャスティングロールにて急冷し、厚さ25μmの非晶シートを作製した。 “B layer-B”:
A polyesterester 6663 manufactured by Eastman Chemical Co. (polyethylene terephthalate glycol, glass transition temperature = 81 ° C., ΔHm = 0 J / g) was used, and the coupler 6663 was kneaded at 260 ° C. with a 40 mmφ single screw extruder and then extruded from the die. Then, it was quenched with a casting roll at about 40 ° C. to produce an amorphous sheet having a thickness of 25 μm.
ポリエステル系樹脂(A)として、東洋紡績社製バイロンGM-443(テレフタル酸:26.5mol%、イソフタル酸:19.8mol%、アジピン酸:4.7mol%、1,4-ブタンジオール:50mol%、ガラス転移温度:26℃、結晶融解熱量ΔHm:22.8J/g)を用い、難燃剤として、日産化学社製メラミン(平均粒径5μm)を用い、フェノキシ樹脂として、ジャパンエポキシレジン社製E4275(ビスフェノールF/ビスフェノールA=75mol%、25mol%)を用いた。
これらバイロンGM-443、メラミン及びE4275を、混合質量比58/40/2の割合でドライブレンドした後、40mmφ同方向二軸押出機を用いて190℃で混練し、T型ダイを付属した単軸の押出機で再度溶融させ、口金よりシート状に押出し、Tダイより押出すと同時に、「B層-A」をキャストロール側から貼り合わせることにより、層構成がA層/B層となる厚さ65μmの積層フィルム(A層=40μm、B層-A=25μm)を得た。
得られた積層フィルムに関して、難燃性の試験を行ない、その結果を表5に示した。 Example 4-1
As a polyester resin (A), Byron GM-443 manufactured by Toyobo Co., Ltd. (terephthalic acid: 26.5 mol%, isophthalic acid: 19.8 mol%, adipic acid: 4.7 mol%, 1,4-butanediol: 50 mol% , Glass transition temperature: 26 ° C., heat of crystal fusion ΔHm: 22.8 J / g), melamine (average particle size: 5 μm) manufactured by Nissan Chemical Co., Ltd. as a flame retardant, and E4275 manufactured by Japan Epoxy Resin Co., Ltd. as a phenoxy resin. (Bisphenol F / bisphenol A = 75 mol%, 25 mol%) was used.
These Byron GM-443, melamine, and E4275 were dry blended at a mixing mass ratio of 58/40/2, and then kneaded at 190 ° C. using a 40 mmφ co-directional twin-screw extruder, and a single die attached with a T-die. It is melted again with a shaft extruder, extruded into a sheet form from a die, extruded from a T die, and at the same time, “B layer-A” is bonded from the cast roll side, so that the layer structure becomes A layer / B layer. A laminated film with a thickness of 65 μm (A layer = 40 μm, B layer−A = 25 μm) was obtained.
The obtained laminated film was tested for flame retardancy, and the results are shown in Table 5.
上記方法で得られたフラットケーブルに関して、A層と錫メッキ銅箔との剥離強度、並びに、耐熱性を測定した結果を表5に示した。 Next, a tin-plated copper foil having a thickness of 150 μm and a width of 10 mm is disposed between the two obtained laminated films (both with the A layer inside), and these are placed on a metal roll (heating) / rubber roll (non-heating). A flat cable was obtained by laminating under conditions of a roll nip pressure of 10 kg / cm (linear pressure) and a laminating speed of 0.5 m / min.
Table 5 shows the results of measuring the peel strength between the A layer and the tin-plated copper foil and the heat resistance of the flat cable obtained by the above method.
また、得られたフラットケーブルを観察し、A層とB層との間に剥離が見られた場合には、前記3項目全てが合格であっても、「×」と評価することにした。 In addition, regarding any one of the flame retardant properties, heat resistance, and adhesion between the A layer and the tin-plated copper foil, the overall evaluation was evaluated as “x” and all items were acceptable. When it was, the overall evaluation was evaluated as “◯”.
Moreover, when the obtained flat cable was observed and peeling was seen between A layer and B layer, even if all the said 3 items passed, it decided to evaluate with "x".
A層の構成において、バイロンGM-443、メラミン及びE4275の混合質量比を55:40:5とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表5に示す。 (Example 4-2)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was 55: 40: 5. A laminated film of A = 40 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 5.
A層の構成において、バイロンGM-443、メラミン及びE4275の混合質量比を50:40:10とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表5に示す。 (Example 4-3)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was set to 50:40:10. A laminated film of A = 40 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 5.
ポリエステル系樹脂(A)として、東洋紡績社製バイロンGA-1300(テレフタル酸:32.8mol%、イソフタル酸:5.1mol%、アジピン酸:12.1mol%、1,4-ブタンジオール:50mol%、ガラス転移温度=-6℃、ΔHm=23.7J/g)を用い、バイロンGA-1300、メラミン及びE4275の混合質量比を50:40:10とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表5に示す。 (Example 4-4)
Byron GA-1300 manufactured by Toyobo Co., Ltd. (terephthalic acid: 32.8 mol%, isophthalic acid: 5.1 mol%, adipic acid: 12.1 mol%, 1,4-butanediol: 50 mol% as the polyester resin (A) Glass transition temperature = −6 ° C., ΔHm = 23.7 J / g), and the mixing mass ratio of Byron GA-1300, melamine and E4275 was set to 50:40:10, and the same as Example 4-1. A laminated film having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was obtained by this method.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 5.
A層の構成において、バイロンGA-1300、メラミン及びE4275の混合質量比を40:40:20とした以外は実施例4-4と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表5に示す。 (Example 4-5)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 4-4 except that the mixing mass ratio of Byron GA-1300, melamine and E4275 was set to 40:40:20. A laminated film of A = 40 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 5.
ポリエステル系樹脂(A)として、東洋紡績社製バイロン30P(テレフタル酸:27.0mol%、セバシン酸:23.0mol%、エチレングリコール:50mol%、ガラス転移温度=-28℃、ΔHm=9.0J/g)を用い、バイロン30P、メラミン及びE4275の混合質量比を50:40:10とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表5に示す。 (Example 4-6)
As the polyester resin (A), Byron 30P manufactured by Toyobo Co., Ltd. (terephthalic acid: 27.0 mol%, sebacic acid: 23.0 mol%, ethylene glycol: 50 mol%, glass transition temperature = −28 ° C., ΔHm = 9.0 J / G) and a thickness of 65 μm (A layer = 25 μm, B layer−A =) by the same method as in Example 4-1, except that the mixing mass ratio of Byron 30P, melamine and E4275 was 50:40:10. 40 μm) laminated film was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 5.
A層の構成において、ポリエステル系樹脂(A)として、上記バイロンGM-443及び30Pの2種類を用い、バイロンGM-443、バイロン30P、メラミン及びE4275の混合質量比を35:20:40:5とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表5に示す。 (Example 4-7)
In the configuration of the A layer, two types of Byron GM-443 and 30P are used as the polyester resin (A), and the mixing mass ratio of Byron GM-443, Byron 30P, melamine and E4275 is 35: 20: 40: 5. A laminated film having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was obtained in the same manner as in Example 4-1, except that
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 5.
A層の構成において、バイロンGM-443、メラミン及びE4275の混合質量比を65:30:5とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表5に示す。 (Example 4-8)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was set to 65: 30: 5. A laminated film of A = 40 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 5.
A層の構成において、バイロンGM-443、メラミン及びE4275の混合質量比を35:60:5とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表6に示す。 (Example 4-9)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was set to 35: 60: 5. A laminated film of A = 40 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 6.
A層の構成において、バイロンGM-443、メラミン及びE4275の混合質量比を78:20:2とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表6に示す。 (Example 4-10)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was 78: 20: 2. A laminated film of A = 40 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 6.
A層の構成において、バイロンGM-443、メラミン及びE4275の混合質量比を28:70:2とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表6に示す。 (Example 4-11)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was 28: 70: 2. A laminated film of A = 40 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 6.
A層の構成において、バイロンGM-443、メラミン及びE4275の混合質量比を18:80:2とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表6に示す。 (Example 4-12)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was 18: 80: 2. A laminated film of A = 40 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 6.
A層の構成において、バイロンGM-443、メラミン及びE4275の混合質量比を35:40:25とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表6に示す。 (Example 4-13)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was set to 35:40:25. A laminated film of A = 40 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 6.
A層として、バイロンGM-443、メラミン及びE4275の混合質量比を30:40:30とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表6に示す。 (Example 4-14)
As the A layer, a thickness of 65 μm (A layer = 25 μm, B layer—A =) was obtained in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was set to 30:40:30. 40 μm) laminated film was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 6.
フェノキシ樹脂として、ジャパンエポキシレジン社製E1256(ビスフェノールA=100mol%)を用い、A層の構成において、バイロンGM-443、メラミン及びE1256の混合質量比を55:40:5とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表6に示す。 (Example 4-15)
Example 1 except that E1256 (bisphenol A = 100 mol%) manufactured by Japan Epoxy Resin Co., Ltd. was used as the phenoxy resin, and the mixing mass ratio of Byron GM-443, melamine and E1256 was 55: 40: 5 in the configuration of layer A A laminated film having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was obtained in the same manner as in 4-1.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 6.
ポリエステル系樹脂(A)として、三菱化学社製GSPla AZ91T(ポリブチレンサクシネート、ガラス転移温度:-30℃、ΔHm:54.0J/g)を用い、A層の構成において、GSPla AZ91T、メラミン及びE4275の混合質量比を55:40:5とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表6に示す。 (Example 4-16)
As the polyester resin (A), GSPla AZ91T (polybutylene succinate, glass transition temperature: −30 ° C., ΔHm: 54.0 J / g) manufactured by Mitsubishi Chemical Corporation was used. In the configuration of the A layer, GSPla AZ91T, melamine and A laminated film having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was obtained in the same manner as in Example 4-1, except that the mixing mass ratio of E4275 was 55: 40: 5.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 6.
A層の構成において、フェノキシ樹脂を用いずに、バイロンGM-443とメラミンを混合質量比60:40でブレンドした後、実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表7に示す。 (Comparative Example 4-1)
In the structure of the A layer, after blending Byron GM-443 and melamine at a mixing mass ratio of 60:40 without using a phenoxy resin, the thickness was 65 μm (A layer = 25 μm, A laminated film of B layer-A = 40 μm was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 7.
A層の構成において、バイロンGM-443、メラミン及びE4275の混合質量比を90:5:5とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表7に示す。 (Comparative Example 4-2)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was 90: 5: 5. A laminated film of A = 40 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 7.
A層の構成において、メラミンの代わりに日産化学工業社製MC-600(メラミンシアヌレート)を用い、バイロンGM-443、MC-601及びE4275を混合質量比55:40:5でブレンドした後、実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表7に示す。 (Comparative Example 4-3)
In the configuration of layer A, MC-600 (melamine cyanurate) manufactured by Nissan Chemical Industries, Ltd. was used instead of melamine, and Byron GM-443, MC-601 and E4275 were blended at a mixing mass ratio of 55: 40: 5, A laminated film having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was obtained in the same manner as in Example 4-1.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 7.
A層に構成において、メラミンの代わりに日本軽金属社製BF013ST(水酸化アルミニウム)を用い、バイロンGM-443、BF013ST及びE4275を混合質量比55:40:5でブレンドした後、実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表7に示す。 (Comparative Example 4-4)
In the configuration of the A layer, BF013ST (aluminum hydroxide) manufactured by Nippon Light Metal Co., Ltd. was used instead of melamine, and Byron GM-443, BF013ST and E4275 were blended at a mixing mass ratio of 55: 40: 5, and then Example 4-1 A laminated film having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was obtained in the same manner as above.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 7.
B層を構成するするフィルムとして「B層-A」の代わりに「B層-B」を用いた以外は、実施例4-2と同様の方法で厚さ65μm(A層=40μm、B層-C=25μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表7に示す。 (Comparative Example 4-5)
A thickness of 65 μm (A layer = 40 μm, B layer) in the same manner as in Example 4-2, except that “B layer-B” was used instead of “B layer-A” as the film constituting the B layer. -C = 25 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 7.
A層の構成において、バイロンGM-443、メラミン及びE4275の混合質量比を60:39.5:0.5とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表7に示す。 (Comparative Example 4-6)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm) in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was set to 60: 39.5: 0.5. , B layer-A = 40 μm).
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 7.
A層の構成において、バイロンGM-443、メラミン及びE4275の混合質量比を25:40:35とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表7に示す。 (Comparative Example 4-7)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was set to 25:40:35. A laminated film of A = 40 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 7.
A層の構成において、バイロンGM-443、メラミン及びE4275の混合質量比を83:15:2とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表7に示す。 (Comparative Example 4-8)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was 83: 15: 2. A laminated film of A = 40 μm) was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 7.
A層として、バイロンGM-443、メラミン及びE4275の混合質量比を13:85:2とした以外は実施例4-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層フィルムを得た。
得られた積層フィルムに関して実施例4-1と同様の評価を行うと共に、実施例4-1と同様にフラットケーブルを作製して評価を行った。結果を表7に示す。 (Comparative Example 4-9)
As the A layer, a thickness of 65 μm (A layer = 25 μm, B layer−A =) was obtained in the same manner as in Example 4-1, except that the mixing mass ratio of Byron GM-443, melamine and E4275 was 13: 85: 2. 40 μm) laminated film was obtained.
The obtained laminated film was evaluated in the same manner as in Example 4-1, and a flat cable was produced and evaluated in the same manner as in Example 4-1. The results are shown in Table 7.
例えば、実施例4-1とフェノキシ樹脂を配合しない比較例4-1とを比較すると、フェノキシ樹脂を配合することで、金属導体との接着性が顕著に高まる上、耐熱性も高まることが判明した。
また、メラミン以外のメラミンシアヌレートを用いた比較例4-3と実施例とを比較すると、メラミンを用いることにより、難燃性を顕著に高めることができることが分かった。メラミンは、燃焼時に不燃性のガスを発生するため、接着層を難燃化することができるばかりか、難燃剤を配合してない外層(B層)をも難燃化することができるため、積層フィルムの難燃性を格別に高めることができる。
なお、上記試験では、銅メッキ錫との接着性を検討したが、フェノキシ樹脂と金属との接着は、金属表面に存在する水分とフェノキシ樹脂との水素結合によるものと考えられるため、銅メッキ錫以外の金属(例えば銀、金、白金、鉄、ステンレス、鋼或いはこれらの合金)に対しても同様の接着性を得ることができるものと考えられる。 From the evaluation results of Examples 4-1 to 16, the VTM-0 in the UL94 vertical combustion test was obtained by adding a phenoxy resin together with melamine to a polyester resin having a specific glass transition temperature in the A layer as an adhesive layer. It was found that in addition to the high flame retardant properties that pass the above, excellent heat resistance and excellent adhesion to metal conductors can be obtained.
For example, comparing Example 4-1 with Comparative Example 4-1, which does not contain a phenoxy resin, it has been found that the addition of a phenoxy resin significantly increases the adhesion to a metal conductor and also increases the heat resistance. did.
Further, when Comparative Example 4-3 using melamine cyanurate other than melamine was compared with Examples, it was found that flame retardancy can be remarkably increased by using melamine. Since melamine generates nonflammable gas when burned, not only can the adhesive layer be flame retardant, but also the outer layer (B layer) that does not contain a flame retardant can also be flame retardant. The flame retardancy of the laminated film can be significantly increased.
In the above test, the adhesion with copper-plated tin was examined. However, the adhesion between the phenoxy resin and the metal is considered to be due to the hydrogen bond between the moisture present on the metal surface and the phenoxy resin. It is considered that the same adhesiveness can be obtained for other metals (for example, silver, gold, platinum, iron, stainless steel, steel or alloys thereof).
かかる観点から、ポリエステル系樹脂(A)のガラス転移温度は、-80℃以上が好ましく、特に-70℃以上、中でも-60℃以上が好ましく、また、30℃以下が好ましく、特に20℃以下、中でも10℃以下であるのが好ましい、と考えることができる。
また、ポリエステル系樹脂(A)の結晶融解熱量ΔHmは5~30J/gであることが好ましく、また、特に8J/g以上、中でも10J/g以上であるのがさらに好ましく、上限値は特に25J/g以下、中でも20J/g以下であるのがさらに好ましい、と考えることができる。 Compared to Example 4-1, Examples 4-4 to 7 use polyester resins (A) having different glass transition temperatures and ΔHm. Considering these results and previous experience, the polyester resin (A) has higher peel strength at lower temperatures (for example, 0 ° C. or lower) when Tg is lower, and crystallinity when ΔHm is higher. It was found that the heat resistance tends to be high because of the high value.
From this viewpoint, the glass transition temperature of the polyester-based resin (A) is preferably −80 ° C. or higher, particularly −70 ° C. or higher, more preferably −60 ° C. or higher, preferably 30 ° C. or lower, particularly 20 ° C. or lower, In particular, it can be considered that the temperature is preferably 10 ° C. or lower.
Further, the heat of crystal fusion ΔHm of the polyester resin (A) is preferably 5 to 30 J / g, more preferably 8 J / g or more, more preferably 10 J / g or more, and the upper limit value is particularly 25 J. / G or less, more preferably 20 J / g or less.
また、ポリエステル系樹脂(B)の結晶融解熱量ΔHmは、40~100J/gであるのが好ましく、下限値としては特に45J/g以上、中でも50J/g以上であるのがさらに好ましく、上限値は特に90J/g以下、中でも80J/g以下であるのがさらに好ましい、と考えることができる。 On the other hand, regarding the polyester-based resin (B), when considering the evaluation results of the above-mentioned Examples and Comparative Examples, particularly the evaluation results of Comparative Example 4-5 and the experience so far, the glass of the polyester-based resin (B) The transition temperature is preferably 50 to 120 ° C., the lower limit is particularly preferably 55 ° C. or higher, more preferably 60 ° C. or higher, and the upper limit is particularly 110 ° C. or lower, especially 100 ° C. or lower. It can be considered more preferable.
The crystal melting heat ΔHm of the polyester-based resin (B) is preferably 40 to 100 J / g, and the lower limit is particularly preferably 45 J / g or more, more preferably 50 J / g or more, and the upper limit. Can be considered to be 90 J / g or less, more preferably 80 J / g or less.
また、A層を構成する樹脂組成物a中に占めるフェノキシ樹脂の割合は、1~30質量%であることが好ましく、下限値は5質量%以上であるのがさらに好ましく、その上限値は20質量%以下であるのがさらに好ましい、と考えることができる。 From the results of the above Examples and Comparative Examples and the experience so far, the blending ratio of melamine in the resin composition a constituting the A layer is preferably 20 to 80% by mass, and the lower limit thereof. Is particularly preferably 30% by mass or more, more preferably 40% by mass or more, and the upper limit is particularly preferably 70% by mass or less, and more preferably 60% by mass or less.
The proportion of the phenoxy resin in the resin composition a constituting the A layer is preferably 1 to 30% by mass, the lower limit is more preferably 5% by mass or more, and the upper limit is 20%. It can be considered that it is more preferable to be not more than mass%.
次に、第5の実施形態に係る実施例及び比較例について説明する。 [Example and Comparative Example of Fifth Embodiment]
Next, examples and comparative examples according to the fifth embodiment will be described.
第3の実施形態に係る実施例と同様に測定及び評価した。 (1) Flame retardancy Measurement and evaluation were performed in the same manner as in the example according to the third embodiment.
第3の実施形態に係る実施例と同様に測定及び評価した。 (2) Tensile strength and tensile elongation Measurement and evaluation were performed in the same manner as in the example according to the third embodiment.
長さ5mm×幅5mm(厚みはそれぞれの試験片により異なる)の評価用サンプルを用いて、JIS K7196に基づき、TMAによる軟化温度の測定を行った。雰囲気温度23℃、相対湿度50%、圧子への圧力0.5N、昇温速度5℃/分にてTMA曲線を測定し、圧子が侵入を始めるよりも低温側に認められる直線部分を高温側に延長し、侵入速度が最大となる部分の接線の低温側への延長との交点を針侵入温度とし、この値から軟化温度を算出した。軟化温度は140℃以上を合格とした。 (3) Heat resistance (softening temperature)
Using a sample for evaluation of 5 mm length × 5 mm width (thickness varies depending on each test piece), the softening temperature was measured by TMA based on JIS K7196. Measure the TMA curve at an ambient temperature of 23 ° C, a relative humidity of 50%, an indenter pressure of 0.5N, and a heating rate of 5 ° C / min. The intersection point with the extension of the tangent of the portion where the penetration speed is maximum to the low temperature side was defined as the needle penetration temperature, and the softening temperature was calculated from this value. The softening temperature passed 140 ° C. or higher.
「B層-1」
ポリエステル系樹脂として三菱化学社製ノバペックス(ポリエチレンテレフタレート、ガラス転移温度=79℃、ΔHm=55J/g)を用い、まず、ノバペックスを直径40mm単軸押出機にて260℃で混練した後、口金から押出し、次いで約40℃のキャスティングロールにて急冷し、厚さ225μmの非晶シートを作製した。次いで、三菱重工株式会社製逐次2軸テンターに通紙し、95℃でMD(長手方向)に延伸倍率で3倍に延伸を行い、続いて、110℃でTD(横手方向)に延伸倍率で3倍に延伸を行った。さらにその後、160℃で15秒熱処理を行い、厚さ25μmの二軸延伸フィルムを得た。 <Preparation of B layer>
"B layer-1"
As a polyester resin, Novapex (polyethylene terephthalate, glass transition temperature = 79 ° C., ΔHm = 55 J / g) manufactured by Mitsubishi Chemical Corporation was used. First, Novapex was kneaded at 260 ° C. with a 40 mm diameter single screw extruder, and then from the die. Extrusion was followed by quenching with a casting roll at about 40 ° C. to produce an amorphous sheet having a thickness of 225 μm. Next, the paper is passed through a sequential biaxial tenter manufactured by Mitsubishi Heavy Industries, Ltd., stretched at 95 ° C. in the MD (longitudinal direction) at a stretch ratio of 3 times, and subsequently at 110 ° C. in the TD (transverse direction) at the stretch ratio. The film was stretched 3 times. Thereafter, a heat treatment was performed at 160 ° C. for 15 seconds to obtain a biaxially stretched film having a thickness of 25 μm.
前記B層-1と同様の方法、条件で厚さ108μmの非晶シートを作製した後、前記B層-1と同様の方法、条件で延伸を行い、厚さ12μmの二軸延伸フィルムを得た。 "B layer-2"
An amorphous sheet having a thickness of 108 μm was prepared under the same method and conditions as the B layer-1, and then stretched under the same methods and conditions as the B layer-1 to obtain a biaxially stretched film having a thickness of 12 μm. It was.
ポリエステル系樹脂として、Nature Works社製NW4032D(ポリ乳酸、ガラス転移温度=55℃、ΔHm=42J/g)を用いた以外は、「B層-1」と同様の方法で厚さ25μmの二軸延伸フィルムを得た。 "B layer-3"
A 25 μm-thick biaxial film in the same manner as “B layer-1” except that NW4032D (polylactic acid, glass transition temperature = 55 ° C., ΔHm = 42 J / g) manufactured by Nature Works is used as the polyester resin. A stretched film was obtained.
A層として、三菱化学社製GSPla AZ91T(ポリブチレンサクシネート、ガラス転移温度=-30℃、ΔHm=54.0J/g)、日産化学工業社製微粉メラミン(メラミン)および日本化成社製TMAIC(トリメタアリルイソシアネート)の混合物を用い、GSPla AZ91T、微粉メラミン、およびTMAICを混合質量比69:30:1の割合でドライブレンドした後、直径40mm同方向二軸押出機を用いて190℃で混練し、55℃のキャスティングロールで厚さ50μmのシート(A層)を得た。次いで、A層の両外層として、B層-1をキャストロール側とニップロール側から貼り合わせることにより、層構成が、B-1/A/B-1となる厚さ100μmの積層体を得た。続いて、積層体に照射線量50kGyで放射線(γ線)を照射した。得られた積層体について、ゲル分率、難燃性、引張強度、伸度、および耐熱性の評価を行った結果を表8に示す。 Example 5-1
As the A layer, GSPla AZ91T (polybutylene succinate, glass transition temperature = −30 ° C., ΔHm = 54.0 J / g) manufactured by Mitsubishi Chemical Corporation, fine powdered melamine (melamine) manufactured by Nissan Chemical Industries, and TMAIC manufactured by Nippon Kasei Co., Ltd. ( GSPla AZ91T, fine melamine, and TMAIC were dry blended at a mixing mass ratio of 69: 30: 1 using a mixture of trimethallyl isocyanate, and then kneaded at 190 ° C. using a 40 mm diameter co-directional twin screw extruder. Then, a sheet (A layer) having a thickness of 50 μm was obtained with a casting roll at 55 ° C. Next, as both outer layers of the A layer, the B layer-1 was bonded from the cast roll side and the nip roll side to obtain a laminate having a layer configuration of B-1 / A / B-1 and a thickness of 100 μm. . Subsequently, the laminate was irradiated with radiation (γ rays) at an irradiation dose of 50 kGy. Table 8 shows the results of evaluating the gel fraction, flame retardancy, tensile strength, elongation, and heat resistance of the obtained laminate.
GSPla AZ91T、微粉メラミン、およびTMAICの混合質量比を59:40:1とした以外は実施例5-1と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Example 5-2)
A laminate was prepared and evaluated in the same manner as in Example 5-1, except that the mixing mass ratio of GSPla AZ91T, fine melamine, and TMAIC was 59: 40: 1. The results are shown in Table 8.
GSPla AZ91T、微粉メラミン、およびTMAICの混合質量比を49:50:1とした以外は実施例5-1と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Example 5-3)
A laminate was prepared and evaluated in the same manner as in Example 5-1, except that the mixing mass ratio of GSPla AZ91T, fine melamine, and TMAIC was 49: 50: 1. The results are shown in Table 8.
GSPla AZ91T、微粉メラミン、およびTMAICの混合質量比を59.5:40:0.5とした以外は実施例5-1と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Example 5-4)
A laminate was prepared and evaluated in the same manner as in Example 5-1, except that the mixing mass ratio of GSPla AZ91T, fine melamine, and TMAIC was set to 59.5: 40: 0.5. The results are shown in Table 8.
GSPla AZ91T、微粉メラミン、およびTMAICの混合質量比を57:40:3とした以外は実施例5-1と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Example 5-5)
A laminate was prepared and evaluated in the same manner as in Example 5-1, except that the mixing mass ratio of GSPla AZ91T, fine melamine, and TMAIC was 57: 40: 3. The results are shown in Table 8.
実施例5-2にて、A層の厚みを20μmとした以外は同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Example 5-6)
A laminate was produced and evaluated in the same manner as in Example 5-2 except that the thickness of the A layer was 20 μm. The results are shown in Table 8.
実施例5-3にて、A層の厚みを70μmとした以外は同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Example 5-7)
A laminate was prepared and evaluated in the same manner as in Example 5-3 except that the thickness of the A layer was changed to 70 μm. The results are shown in Table 8.
実施例5-2にて、A層の厚みを30μmとし、B層としてB-2を用いた以外は同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Example 5-8)
A laminate was prepared and evaluated in the same manner as in Example 5-2 except that the thickness of the A layer was 30 μm and B-2 was used as the B layer. The results are shown in Table 8.
GSPla AZ91T、微粉メラミン、およびTMAICの混合質量比を39:60:1、A層の厚みを35μmとし、B層としてB層-2を用いた以外は実施例5-1と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Example 5-9)
GSPla AZ91T, fine melamine, and TMAIC were mixed in the same manner as in Example 5-1, except that the mixing mass ratio was 39: 60: 1, the thickness of layer A was 35 μm, and layer B-2 was used as layer B. The body was prepared and evaluated. The results are shown in Table 8.
ポリエステル系樹脂(A)として三菱化学社製GSPla AD92W(ポリブチレンサクシネート・アジペート共重合体、ガラス転移温度=-40℃、ΔHm=35J/g)を用い、GSPla AD92W、微粉メラミンおよびTMAICを混合質量比59:40:1でドライブレンドした後、実施例5-1と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Example 5-10)
GSPla AD92W (polybutylene succinate / adipate copolymer, glass transition temperature = −40 ° C., ΔHm = 35 J / g) manufactured by Mitsubishi Chemical Corporation as polyester resin (A) is mixed with GSPla AD92W, fine melamine and TMAIC After dry blending at a mass ratio of 59: 40: 1, a laminate was produced and evaluated in the same manner as in Example 5-1. The results are shown in Table 8.
GSPla AD92W、微粉メラミン、およびTMAICの混合質量比を49:50:1、A層の厚みを70μmとした以外は実施例5-1と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Example 5-11)
A laminate was prepared and evaluated in the same manner as in Example 5-1, except that the mixing mass ratio of GSPla AD92W, fine melamine, and TMAIC was 49: 50: 1, and the thickness of the A layer was 70 μm. The results are shown in Table 8.
架橋剤として、四国化成工業社製DA-MGIC(ジアリルモノグリシジルイソシアネート)を用い、GSPla AZ91T、微粉メラミン、およびDA-MGICの混合質量比を59:40:1とした以外は実施例5-1と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Example 5-12)
Example 5-1 except that DA-MGIC (diallyl monoglycidyl isocyanate) manufactured by Shikoku Kasei Kogyo Co., Ltd. was used as the crosslinking agent, and the mixing mass ratio of GSPla AZ91T, fine melamine, and DA-MGIC was 59: 40: 1. A laminate was prepared and evaluated in the same manner as described above. The results are shown in Table 8.
GSPla AZ91T、微粉メラミン、およびTMAICの混合質量比を84:15:1とした以外は実施例5-1と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Comparative Example 5-1)
A laminate was prepared and evaluated in the same manner as in Example 5-1, except that the mixing mass ratio of GSPla AZ91T, fine melamine, and TMAIC was 84: 15: 1. The results are shown in Table 8.
GSPla AZ91T、微粉メラミン、およびTMAICの混合質量比を39:60:1、A層の厚みを150μmとした以外は実施例5-1と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Comparative Example 5-2)
A laminate was prepared and evaluated in the same manner as in Example 5-1, except that the mixing mass ratio of GSPla AZ91T, fine melamine, and TMAIC was 39: 60: 1, and the thickness of the A layer was 150 μm. The results are shown in Table 8.
実施例5-2にて、架橋剤を配合せずに積層体の作製、評価を行った結果を表8に示す。 (Comparative Example 5-3)
Table 8 shows the results of preparation and evaluation of the laminate in Example 5-2 without adding a crosslinking agent.
実施例5-2と同様のA層を作製し、B層を貼り合わせていない単層体の作製、評価を行った。結果を表8に示す。 (Comparative Example 5-4)
A layer A similar to that in Example 5-2 was prepared, and a single layer body in which the B layer was not bonded was prepared and evaluated. The results are shown in Table 8.
実施例5-3にて、A層の厚みを10μmとした以外は同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Comparative Example 5-5)
A laminate was prepared and evaluated in the same manner as in Example 5-3 except that the thickness of the A layer was changed to 10 μm. The results are shown in Table 8.
メラミンの代わりに日産化学工業社製MC-860(メラミンシアヌレート)を用い、GSPla AZ91T、MC-860、およびTMAICの混合質量比を59:40:1とした以外は実施例5-1と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Comparative Example 5-6)
Example 5-1 except that MC-860 (melamine cyanurate) manufactured by Nissan Chemical Industries, Ltd. was used instead of melamine, and the mixing mass ratio of GSPla AZ91T, MC-860, and TMAIC was set to 59: 40: 1. The laminate was prepared and evaluated by the method described above. The results are shown in Table 8.
メラミンの代わりに昭和電工社製H42S(水酸化アルミニウム)を用い、GSPlaAZ91T、H42S、およびTMAICの混合質量比を59:40:1とした以外は実施例5-1と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Comparative Example 5-7)
The laminate was prepared in the same manner as in Example 5-1, except that H42S (aluminum hydroxide) manufactured by Showa Denko KK was used instead of melamine, and the mixing mass ratio of GSPlaAZ91T, H42S, and TMAIC was set to 59: 40: 1. Fabrication and evaluation were performed. The results are shown in Table 8.
A層として、東洋紡績社製バイロン(登録商標)GA1310(ポリエステル系共重合体(テレフタル酸35mol%、イソフタル酸15mol%、1,4-ブタンジオール50mol%)、ガラス転移温度=27℃、ΔHm=26.1J/g)を用い、GA1310、微粉メラミン、およびTMAICの混合質量比を49:50:1とした以外は実施例5-3と同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Comparative Example 5-8)
As layer A, Toyobo Co., Ltd. Byron (registered trademark) GA1310 (polyester copolymer (35 mol% terephthalic acid, 15 mol% isophthalic acid, 50 mol% 1,4-butanediol), glass transition temperature = 27 ° C, ΔHm = 26.1 J / g), and a laminate was prepared and evaluated in the same manner as in Example 5-3 except that the mixing mass ratio of GA1310, fine melamine, and TMAIC was 49: 50: 1. The results are shown in Table 8.
実施例5-3にて、B層としてB層-3を用いた以外は同様の方法で積層体の作製、評価を行った。結果を表8に示す。 (Comparative Example 5-9)
A laminate was prepared and evaluated in the same manner as in Example 5-3 except that B layer-3 was used as the B layer. The results are shown in Table 8.
次に、第6の実施形態に係る実施例及び比較例について説明する。 [Example and Comparative Example of Sixth Embodiment]
Next, examples and comparative examples according to the sixth embodiment will be described.
長さ200mm×幅50mm(厚みはそれぞれの試験片により異なる)の評価用サンプル(積層体)を用いて、Underwriters Laboratories社の安全標準UL94垂直燃焼試験の手順に基づき、試験回数5回にて燃焼試験を実施した。
UL94垂直燃焼試験UL94VTMの判定基準に基づき、VTM-0規格を満たすものを○とし、満たさないものを×とした。 (1) Flame retardancy (UL94VTM) (laminate)
Combustion was performed 5 times based on the safety standard UL94 vertical combustion test procedure of Underwriters Laboratories using an evaluation sample (laminate) of length 200 mm x width 50 mm (thickness varies depending on each specimen). The test was conducted.
Based on the criteria of UL94 vertical combustion test UL94VTM, those satisfying the VTM-0 standard were marked with ◯, and those not satisfying were marked with x.
長さ600mm×幅19mm(厚みはそれぞれの試験片により異なる)の評価用サンプル(フラットケーブル)を、UL1581VW-1規格の燃焼試験方法に基づき、チリルバーナーを用いて15秒着火、15秒休止を5回繰り返し、試験片の燃焼時間、インジケータの損傷割合、ドリップによる脱脂綿の着火有無により判定を行った。燃焼時間が60秒以下、インジケータの損傷割合が25%以下、ドリップによる脱脂綿の着火がないものをUL1581VW-1合格とした。表9には、合格のものを○、不合格のものを×と表記した。 (2) Flame resistance (UL1581VW-1) (flat cable)
A sample for evaluation (flat cable) measuring 600 mm long × 19 mm wide (thickness varies depending on each test piece) is ignited for 15 seconds using a tyryl burner and 5 seconds rest for 15 seconds based on the UL 1581VW-1 standard combustion test method. The determination was made by repeating the test times, the burning time of the test piece, the damage ratio of the indicator, and whether or not the absorbent cotton was ignited by drip. UL1581VW-1 passed when the burning time was 60 seconds or less, the indicator damage rate was 25% or less, and the absorbent cotton was not ignited by drip. In Table 9, “Obtained” was marked with “OK”, and “X” was rejected.
長さ600mm×幅30mm(厚みはそれぞれの試験片により異なる)の評価用サンプル(フラットケーブル)を、ベーキング試験装置(大栄科学精器製作所製DKS-5S)内に静置し、120℃で24時間加熱した。
加熱後のサンプルの外観を目視にて観察し、銅箔の剥離、フラットケーブルの収縮、シワ、変形等がないものを「○」、銅箔の剥離、フラットケーブルの収縮、シワ、変形等が生じているものを「×」と評価した。 (3) Heat resistance A sample for evaluation (flat cable) having a length of 600 mm × width of 30 mm (thickness varies depending on each test piece) is left in a baking test apparatus (DKS-5S manufactured by Daiei Kagaku Seiki Seisakusho). And heated at 120 ° C. for 24 hours.
Visually observe the appearance of the sample after heating, “○” if there is no copper foil peeling, flat cable shrinkage, wrinkles, deformation, etc., copper foil peeling, flat cable shrinkage, wrinkles, deformation, etc. What was produced was evaluated as “x”.
長さ600mm×幅30mm(厚みはそれぞれの試験片により異なる)の評価用サンプル(フラットケーブル)を、180度折り曲げた時の外観を目視にて観察し、銅箔と接着剤の剥離やクラックが生じていないものを「○」、生じているものを「×」と評価した。 (4) Bendability The appearance when a sample for evaluation (flat cable) having a length of 600 mm x a width of 30 mm (thickness varies depending on each test piece) is bent 180 degrees is visually observed, and a copper foil and an adhesive The case where no peeling or cracking occurred was evaluated as “◯”, and the case where it was generated was evaluated as “X”.
B層を構成するフィルムとして、次の2種類のフィルム(「B層-A」「B層-B」)を作製し用意した。 <Preparation of B layer>
The following two types of films (“B layer-A” and “B layer-B”) were prepared and prepared as the film constituting the B layer.
ポリエステル系樹脂として三菱化学社製ノバペックス(登録商標)(ポリエチレンテレフタレート、ガラス転移温度=79℃、ΔHm=55J/g)を用い、まず、ノバペックスを40mm直径単軸押出機にて260℃で混練した後、口金から押出し、次いで約40℃のキャスティングロールにて急冷し、厚さ225μmの非晶シートを作製した。次いで、三菱重工株式会社製逐次2軸テンターに通紙し、95℃でMD(長手方向)に延伸倍率で3倍に延伸を行い、続いて、110℃でTD(横手方向)に延伸倍率で3倍に延伸を行った。さらにその後、160℃で15秒熱処理を行い、厚さ25μmの二軸延伸フィルムを得た。 “B layer-A”:
Novapex (registered trademark) manufactured by Mitsubishi Chemical Corporation (polyethylene terephthalate, glass transition temperature = 79 ° C., ΔHm = 55 J / g) was used as the polyester-based resin. First, Novapex was kneaded at 260 ° C. with a 40 mm diameter single screw extruder. Then, it extruded from the nozzle | cap | die, and then rapidly cooled with a casting roll at about 40 ° C. to produce an amorphous sheet having a thickness of 225 μm. Next, the paper is passed through a sequential biaxial tenter manufactured by Mitsubishi Heavy Industries, Ltd., stretched at 95 ° C. in the MD (longitudinal direction) at a stretch ratio of 3 times, and subsequently at 110 ° C. in the TD (transverse direction) at the stretch ratio. The film was stretched 3 times. Thereafter, a heat treatment was performed at 160 ° C. for 15 seconds to obtain a biaxially stretched film having a thickness of 25 μm.
ポリエステル系樹脂としてイーストマンケミカル社製coplyester6763(ポリエチレンテレフタレートグリコール、ガラス転移温度=81℃、ΔHm=0J/g)を用い、coplyester6763を40mm直径単軸押出機にて260℃で混練した後、口金から押出し、次いで約40℃のキャスティングロールにて急冷し、厚さ25μmの非晶シートを作製した。 “B layer-B”:
Using a polyester 6673 (Esterman Chemical Co., Ltd., polyethylene terephthalate glycol, glass transition temperature = 81 ° C., ΔHm = 0 J / g) as a polyester-based resin, the coupler 6663 was kneaded at 260 ° C. with a 40 mm diameter single screw extruder, and then from the die. Extrusion was followed by quenching with a casting roll at about 40 ° C. to produce an amorphous sheet having a thickness of 25 μm.
ポリエステル系樹脂(A)として、東洋紡績社製バイロン(登録商標)GM-480(テレフタル酸:45mol%、セバシン酸:5mol%、1,4-ブタンジオール:50mol%、ガラス転移温度:-2℃、結晶融解熱量ΔHm:24.6J/g)を用い、難燃剤として、日産化学社製微粉メラミン(平均粒径5μm)を用い、炭化促進剤として、巴工業社製PKHB(フェノキシ樹脂)を用いた。
これらバイロンGM-480、メラミンおよびPKHBを、混合質量比55:40:5の割合でドライブレンドした後、40mm直径同方向二軸押出機を用いて190℃で混練し、T型ダイを付属した単軸の押出機で再度溶融させ、口金よりシート状に押出し、Tダイより押出すと同時に、「B層-A」をキャストロール側から貼り合わせることにより、層構成がA層/B層となる厚さ65μmの積層体(A層=40μm、B層-A=25μm)を得た。 Example 6-1
As a polyester resin (A), Byron (registered trademark) GM-480 manufactured by Toyobo Co., Ltd. (terephthalic acid: 45 mol%, sebacic acid: 5 mol%, 1,4-butanediol: 50 mol%, glass transition temperature: −2 ° C. , Crystal melting heat quantity ΔHm: 24.6 J / g), Nissan Chemical Co., Ltd. fine melamine (average particle size 5 μm) is used as a flame retardant, Sakai Kogyo Co., Ltd. PKHB (phenoxy resin) is used as a carbonization accelerator It was.
These Byron GM-480, melamine and PKHB were dry blended at a mixing mass ratio of 55: 40: 5, then kneaded at 190 ° C. using a 40 mm diameter co-directional twin screw extruder, and attached with a T-die. It is melted again with a single screw extruder, extruded into a sheet form from a die, extruded from a T-die, and at the same time, “B layer-A” is bonded from the cast roll side, so that the layer structure becomes A layer / B layer. A laminate having a thickness of 65 μm (A layer = 40 μm, B layer−A = 25 μm) was obtained.
上記方法で得られた積層体に関して難燃性(UL94VTM)、フラットケーブルに関して、難燃性(UL1581VW-1)、耐熱性、並びに、折り曲げ性を評価した結果を以下表9に示した。 Next, a tin-plated copper foil having a thickness of 150 μm and a width of 10 mm is placed between the two obtained laminates (both with the A layer inside), and these are made of a metal roll (heating) / rubber roll (non-heating). A flat cable was obtained by laminating under conditions of a roll nip pressure of 10 kg / cm (linear pressure) and a laminating speed of 0.5 m / min.
Table 9 shows the results of evaluation of flame retardancy (UL94VTM) for the laminate obtained by the above method, flame retardancy (UL1581VW-1), heat resistance, and bendability for the flat cable.
また、得られたフラットケーブルを観察し、A層とB層との間に剥離が見られた場合には、前記3項目全てが合格であっても、「×」と評価することにした。 In addition, regarding flame retardancy, heat resistance, and bendability, if even one of them fails, the overall evaluation is evaluated as “×”, and if all items are acceptable, the overall evaluation is “○”. evaluated.
Moreover, when the obtained flat cable was observed and peeling was seen between A layer and B layer, even if all the said 3 items passed, it decided to evaluate with "x".
A層の構成において、バイロンGM-480、メラミンおよびPKHBの混合質量比を50:40:10とした以外は実施例6-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Example 6-2)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) in the same manner as in Example 6-1 except that the mixing mass ratio of Byron GM-480, melamine and PKHB was 50:40:10. A laminate of A = 40 μm) was obtained. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
炭化促進剤として、日産化学工業社製MC-600(メラミンシアヌレート)を用い、A層の構成において、バイロンGM-480、メラミンおよびMC-600の混合質量比を40:40:20とした以外は実施例6-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Example 6-3)
MC-600 (melamine cyanurate) manufactured by Nissan Chemical Industries, Ltd. was used as a carbonization accelerator, and the mixing mass ratio of Byron GM-480, melamine and MC-600 was set to 40:40:20 in the configuration of layer A Obtained a laminate having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) in the same manner as in Example 6-1. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
炭化促進剤として、純正化学社製ペンタエリスリトールを用い、A層の構成において、バイロンGM-480、メラミンおよびペンタエリスリトールの混合質量比を40:40:20とした以外は実施例6-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Example 6-4)
The same as Example 6-1 except that pentaerythritol manufactured by Junsei Chemical Co., Ltd. was used as the carbonization accelerator, and the mixing mass ratio of Byron GM-480, melamine and pentaerythritol was 40:40:20 in the configuration of layer A. In this way, a laminate having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was obtained. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
炭化促進剤として、ナカライテスク社製水酸化アルミニウムを用い、A層の構成において、バイロンGM-480、メラミンおよび水酸化アルミニウムの混合質量比を50:40:10とした以外は実施例6-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Example 6-5)
Example 6-1 except that aluminum hydroxide manufactured by Nacalai Tesque was used as the carbonization accelerator, and the mixing mass ratio of Byron GM-480, melamine and aluminum hydroxide was 50:40:10 in the configuration of layer A. A layered product having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was obtained in the same manner as above. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
A層の構成において、バイロンGM-480、メラミンおよびMC-600の混合質量比を50:30:20とした以外は同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Example 6-6)
65 μm thickness (A layer = 25 μm, B layer−A = 40 μm) in the same manner except that the mixing mass ratio of Byron GM-480, melamine and MC-600 was 50:30:20 A laminate was obtained. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
A層の構成において、バイロンGM-480、メラミンおよびPKHBの混合質量比を35:60:5とした以外は同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Example 6-7)
A layer having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was formed in the same manner except that the mixing mass ratio of Byron GM-480, melamine and PKHB was set to 35: 60: 5. Got the body. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
A層の構成において、バイロンGM-480、メラミン、PKHBおよびMC-600の混合質量比を35:40:5:20とした以外は同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Example 6-8)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−) except that the mixing mass ratio of Byron GM-480, melamine, PKHB and MC-600 was set to 35: 40: 5: 20. A laminate of A = 40 μm) was obtained. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
A層の構成において、バイロンGM-480、メラミン、PKHBおよびペンタエリスリトールの混合質量比を45:40:5:10とした以外は同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Example 6-9)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer−A) except that the mixing mass ratio of Byron GM-480, melamine, PKHB and pentaerythritol was 45: 40: 5: 10. = 40 μm) was obtained. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
ポリエステル系樹脂(A)として、東洋紡績社製バイロン(登録商標)GM-443(テレフタル酸:27mol%、イソフタル酸:19mol%、アジピン酸:4mol%、1,4-ブタンジオール:50mol%、ガラス転移温度:26℃、結晶融解熱量ΔHm:22.8J/g)を用い、A層の構成において、バイロンGM-443、メラミンおよびMC-600の混合質量比を40:40:20とした以外は実施例6-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Example 6-10)
As a polyester resin (A), Byron (registered trademark) GM-443 manufactured by Toyobo Co., Ltd. (terephthalic acid: 27 mol%, isophthalic acid: 19 mol%, adipic acid: 4 mol%, 1,4-butanediol: 50 mol%, glass Transition temperature: 26 ° C., heat of crystal fusion ΔHm: 22.8 J / g), and in the configuration of layer A, the mixing mass ratio of Byron GM-443, melamine and MC-600 was 40:40:20 A laminate having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was obtained in the same manner as in Example 6-1. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
ポリエステル系樹脂(A)として、東洋紡績社製バイロン(登録商標)30P(テレフタル酸:27mol%、セバシン酸:23mol%、エチレングリコール:50mol%、ガラス転移温度:-28℃、結晶融解熱量ΔHm:2.0J/g)を用い、A層の構成において、バイロン30P、メラミンおよびMC-600の混合質量比を40:40:20とした以外は実施例6-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。
得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Example 6-11)
As the polyester resin (A), Byron (registered trademark) 30P manufactured by Toyobo Co., Ltd. (terephthalic acid: 27 mol%, sebacic acid: 23 mol%, ethylene glycol: 50 mol%, glass transition temperature: −28 ° C., heat of crystal melting ΔHm: A thickness of 65 μm in the same manner as in Example 6-1 except that the mixing mass ratio of Byron 30P, melamine and MC-600 was set to 40:40:20 in the configuration of layer A using 2.0 J / g) A laminate of (A layer = 25 μm, B layer−A = 40 μm) was obtained. Next, a flat cable was produced in the same manner as in Example 6-1.
The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
A層の構成において、バイロンGM-480、メラミンおよびMC-600の混合質量比を70:10:20とした以外は同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Comparative Example 6-1)
65 μm thickness (A layer = 25 μm, B layer−A = 40 μm) in the same manner except that the mixing mass ratio of Byron GM-480, melamine and MC-600 was set to 70:10:20 A laminate was obtained. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
A層の構成において、バイロンGM-480、メラミンおよびPKHBの混合質量比を5:90:5とした以外は同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。
得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Comparative Example 6-2)
A layer having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was formed in the same manner except that the mixing mass ratio of Byron GM-480, melamine and PKHB was changed to 5: 90: 5 in the configuration of the A layer. Got the body. Next, a flat cable was produced in the same manner as in Example 6-1.
The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
A層の構成において、バイロンGM-480、およびメラミンを混合質量比60:40でブレンドした以外は同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Comparative Example 6-3)
A laminate having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was obtained in the same manner except that Byron GM-480 and melamine were blended at a mixing mass ratio of 60:40 in the configuration of the A layer. It was. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
A層の構成において、バイロンGM-480、メラミンおよびMC-600(メラミンシアヌレート)の混合質量比を40:10:50とした以外は同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Comparative Example 6-4)
In the configuration of the A layer, the thickness was 65 μm (A layer = 25 μm, B layer) except that the mixing mass ratio of Byron GM-480, melamine and MC-600 (melamine cyanurate) was 40:10:50. A laminate of −A = 40 μm was obtained. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
B層を構成するするフィルムとして「B層-A」の代わりに「B層-B」を用いた以外は、実施例6-3と同様の方法で厚さ65μm(A層=40μm、B層-C=25μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Comparative Example 6-5)
A thickness of 65 μm (A layer = 40 μm, B layer) in the same manner as in Example 6-3, except that “B layer-B” was used instead of “B layer-A” as the film constituting the B layer. A laminate of −C = 25 μm was obtained. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
ポリエステル系樹脂(A)として、NatureWorks社製NW4032D(ポリ乳酸、ガラス転移温度:55℃、結晶融解熱量ΔHm:42.5J/g)を用い、A層の構成において、NW4032D、メラミンおよびMC-600の混合質量比を40:40:20とした以外は実施例6-1と同様の方法で厚さ65μm(A層=25μm、B層-A=40μm)の積層体を得た。次いで、実施例6-1と同様の方法でフラットケーブルを作製した。得られた積層体、フラットケーブルを用いて、実施例6-1と同様の評価を行った。結果を表9に示す。 (Comparative Example 6-6)
NW4032D (polylactic acid, glass transition temperature: 55 ° C., heat of crystal fusion ΔHm: 42.5 J / g) manufactured by NatureWorks is used as the polyester resin (A), and NW4032D, melamine and MC-600 are used in the configuration of the A layer. A laminate having a thickness of 65 μm (A layer = 25 μm, B layer−A = 40 μm) was obtained in the same manner as in Example 6-1 except that the mixing mass ratio was 40:40:20. Next, a flat cable was produced in the same manner as in Example 6-1. The same evaluation as in Example 6-1 was performed using the obtained laminate and flat cable. The results are shown in Table 9.
Claims (19)
- ガラス転移温度Tgが40℃以下であり、結晶融解温度Tmが140℃~190℃であるポリエステル系樹脂と、メラミンとの混合物を含有する難燃性ポリエステル系樹脂組成物であって、
難燃性ポリエステル系樹脂組成物中のメラミンの割合が10~80質量%であることを特徴とする難燃性ポリエステル系樹脂組成物。 A flame-retardant polyester resin composition comprising a mixture of a polyester resin having a glass transition temperature Tg of 40 ° C. or lower and a crystal melting temperature Tm of 140 ° C. to 190 ° C. and melamine,
A flame retardant polyester resin composition, wherein the ratio of melamine in the flame retardant polyester resin composition is 10 to 80% by mass. - ガラス転移温度Tgが-20℃~40℃であり、結晶融解温度Tmが140℃~190℃であるポリエステル系樹脂と、ガラス転移温度Tgが-100℃以上、-20℃未満であり、結晶融解温度Tmが100℃以上、140℃未満であるポリエステル系樹脂と、メラミンとの混合物を含有する難燃性ポリエステル系樹脂組成物であり、
難燃性ポリエステル系樹脂組成物中のメラミンの割合が20~60質量%であり、且つ、前者のポリエステル系樹脂と後者のポリエステル系樹脂との質量割合が90:10~30:70であることを特徴とする請求項1記載の難燃性ポリエステル系樹脂組成物。 A polyester resin having a glass transition temperature Tg of −20 ° C. to 40 ° C. and a crystal melting temperature Tm of 140 ° C. to 190 ° C., and a glass transition temperature Tg of −100 ° C. or more and less than −20 ° C. A flame retardant polyester resin composition containing a mixture of a polyester resin having a temperature Tm of 100 ° C. or more and less than 140 ° C. and melamine,
The ratio of melamine in the flame-retardant polyester resin composition is 20 to 60% by mass, and the mass ratio of the former polyester resin and the latter polyester resin is 90:10 to 30:70. The flame-retardant polyester-based resin composition according to claim 1. - 前記ポリエステル系樹脂が、多価カルボン酸成分として、テレフタル酸を50~90mol%含有し、かつ、多価アルコール成分として、1,4-ブタンジオール、エチレングリコール、及び、ジエチレングリコールを合計で70~100mol%含有することを特徴とする請求項1記載の難燃性ポリエステル系樹脂組成物。 The polyester resin contains 50 to 90 mol% of terephthalic acid as a polyvalent carboxylic acid component, and 70 to 100 mol in total of 1,4-butanediol, ethylene glycol, and diethylene glycol as polyhydric alcohol components. % Flame retardant polyester-based resin composition according to claim 1.
- 前記難燃性ポリエステル系樹脂組成物が、フェノキシ樹脂を含有することを特徴とする請求項1~3の何れかに記載の難燃性ポリエステル系樹脂組成物。 4. The flame retardant polyester resin composition according to claim 1, wherein the flame retardant polyester resin composition contains a phenoxy resin.
- ポリエステル系樹脂、メラミン、及び、フェノキシ樹脂の混合物を含有する難燃性ポリエステル系樹脂組成物であり、
ポリエステル系樹脂が、多価カルボン酸成分として、テレフタル酸を50~90mol%含有し、かつ、多価アルコール成分として、1,4-ブタンジオール、エチレングリコール、及び、ジエチレングリコールを合計で70~100mol%含有することを第1の特徴とし、
難燃性ポリエステル系樹脂組成物に占めるメラミンの割合が10~60質量%であり、フェノキシ樹脂の割合が1~25質量%であることを第2の特徴とする請求項4に記載の難燃性ポリエステル系樹脂組成物。 A flame retardant polyester resin composition containing a mixture of polyester resin, melamine, and phenoxy resin,
The polyester resin contains 50 to 90 mol% of terephthalic acid as the polyvalent carboxylic acid component, and 70 to 100 mol% in total of 1,4-butanediol, ethylene glycol, and diethylene glycol as the polyhydric alcohol component. It contains as the first feature,
The flame retardant according to claim 4, wherein the proportion of melamine in the flame retardant polyester resin composition is 10 to 60% by mass and the proportion of phenoxy resin is 1 to 25% by mass. Polyester resin composition. - 前記難燃性ポリエステル系樹脂組成物が、炭化促進剤を含有することを特徴とする請求項1に記載の難燃性ポリエステル系樹脂組成物。 The flame retardant polyester resin composition according to claim 1, wherein the flame retardant polyester resin composition contains a carbonization accelerator.
- 前記炭化促進剤が、水酸基を有する化合物であることを特徴とする請求項6記載の難燃性ポリエステル系樹脂組成物。 The flame retardant polyester resin composition according to claim 6, wherein the carbonization accelerator is a compound having a hydroxyl group.
- 前記炭化促進剤が、メラミンシアヌレートであることを特徴とする請求項7記載の難燃性ポリエステル系樹脂組成物。 The flame retardant polyester resin composition according to claim 7, wherein the carbonization accelerator is melamine cyanurate.
- 前記難燃性ポリエステル系樹脂組成物が、架橋剤を含有することを特徴とする請求項1に記載の難燃性ポリエステル系樹脂組成物。 The flame retardant polyester resin composition according to claim 1, wherein the flame retardant polyester resin composition contains a crosslinking agent.
- 前記架橋剤が、トリメタアリルイソシアネートであることを特徴とする請求項9に記載の難燃性ポリエステル系樹脂組成物。 The flame retardant polyester resin composition according to claim 9, wherein the crosslinking agent is trimethallyl isocyanate.
- 前記請求項1~10の何れかに記載の難燃性ポリエステル系樹脂組成物からなる難燃性樹脂体。 A flame-retardant resin body comprising the flame-retardant polyester resin composition according to any one of claims 1 to 10.
- 前記請求項1~10の何れかに記載の難燃性ポリエステル系樹脂組成物からなる樹脂層の少なくとも1表面上に、他の樹脂層を有する難燃性積層体。 A flame retardant laminate having another resin layer on at least one surface of a resin layer comprising the flame retardant polyester resin composition according to any one of claims 1 to 10.
- 前記請求項1~10の何れかに記載の樹脂組成物からなる樹脂層の樹脂層の少なくとも1表面上に、ガラス転移温度が50℃以上であり、結晶融解熱量ΔHmが40J/g以上であるポリエステル系樹脂を含有する樹脂組成物からなる他の樹脂層を有する難燃性樹脂積層体。 The glass transition temperature is 50 ° C. or higher and the heat of crystal fusion ΔHm is 40 J / g or higher on at least one surface of the resin layer of the resin layer comprising the resin composition according to claim 1. A flame-retardant resin laminate having another resin layer comprising a resin composition containing a polyester resin.
- ガラス転移温度が-80~30℃であるポリエステル系樹脂、メラミン、及び、フェノキシ樹脂の混合物を主成分とする樹脂組成物aからなるA層を有し、当該A層上に、ガラス転移温度が50~120℃であり、結晶融解熱量ΔHmが40~100J/gであるポリエステル系樹脂を主成分とする樹脂組成物bからなるB層を有する樹脂積層体であり、
A層を構成する樹脂組成物a中に占めるメラミンの割合が20~80質量%であり、かつ、樹脂組成物a中に占めるフェノキシ樹脂の割合が1~30質量%であることを特徴とする請求項12又は13に記載の難燃性樹脂積層体。 It has an A layer composed of a resin composition a composed mainly of a mixture of a polyester resin having a glass transition temperature of −80 to 30 ° C., a melamine, and a phenoxy resin, and the glass transition temperature is on the A layer. A resin laminate having a B layer composed of a resin composition b mainly composed of a polyester-based resin having a heat of crystal melting ΔHm of 40 to 100 J / g at 50 to 120 ° C .;
The proportion of melamine in the resin composition a constituting the layer A is 20 to 80% by mass, and the proportion of phenoxy resin in the resin composition a is 1 to 30% by mass. The flame-retardant resin laminate according to claim 12 or 13. - ガラス転移温度が30℃以下であるポリエステル系樹脂、メラミンおよび炭化促進剤の混合物を主成分とする樹脂組成物aからなるA層を有し、
当該A層上に、ガラス転移温度が50~120℃であり、結晶融解熱量ΔHmが40~100J/gであるポリエステル系樹脂を主成分とする樹脂組成物bからなるB層を有する積層体であり、
A層を構成する樹脂組成物a中に占めるメラミンの割合が20~80質量%であり、かつ、樹脂組成物a中に占める炭化促進剤の割合が1~30質量%であることを特徴とする請求項12又は13に記載の難燃性樹脂積層体。 Having a layer A composed of a resin composition a whose main component is a mixture of a polyester-based resin having a glass transition temperature of 30 ° C. or less, a melamine and a carbonization accelerator,
On the A layer, a laminate having a B layer composed of a resin composition b mainly composed of a polyester resin having a glass transition temperature of 50 to 120 ° C. and a crystal melting heat ΔHm of 40 to 100 J / g. Yes,
The ratio of the melamine in the resin composition a constituting the layer A is 20 to 80% by mass, and the ratio of the carbonization accelerator in the resin composition a is 1 to 30% by mass. The flame-retardant resin laminate according to claim 12 or 13. - 前記請求項14又は15の難燃性樹脂積層体が金属接着用であることを特徴とする難燃性樹脂積層体。 A flame retardant resin laminate according to claim 14 or 15, wherein the flame retardant resin laminate is for metal bonding.
- ガラス転移温度が20℃以下のポリエステル系樹脂、メラミンおよび架橋剤の混合物を主成分とするA層の少なくとも片側に、ガラス転移温度が60℃以上のポリエステル系樹脂を主成分とするB層を有する積層体であり、
前記積層体のゲル分率が15質量%以上、55質量%以下でありかつ積層体に占めるメラミンの割合が10質量%以上、40質量%以下であることを特徴とする請求項12又は13に記載の難燃性樹脂積層体。 At least one side of the A layer mainly comprising a mixture of a polyester resin having a glass transition temperature of 20 ° C. or lower, a melamine and a crosslinking agent has a B layer having a polyester resin having a glass transition temperature of 60 ° C. or higher as a main component. A laminate,
The gel fraction of the laminate is 15% by mass or more and 55% by mass or less, and the proportion of melamine in the laminate is 10% by mass or more and 40% by mass or less. The flame-retardant resin laminate described. - 請求項1~10の何れかに記載の難燃性ポリエステル系樹脂組成物を用いた配線ケーブル。 A wiring cable using the flame-retardant polyester resin composition according to any one of claims 1 to 10.
- 請求項11に記載の難燃性樹脂シート又は請求項12~17の何れかに記載の難燃性樹脂積層体を用いた配線ケーブル。
A wiring cable using the flame retardant resin sheet according to claim 11 or the flame retardant resin laminate according to any one of claims 12 to 17.